  ALTECH PA6 A 1000/518 IM | PA6-I | ALBIS Plastic GmbH
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 2300 / 1400 MPa ISO 527-1/-2
Stress at break 60 / - MPa ISO 527-1/-2
Strain at break 3.9 / - % ISO 527-1/-2
Charpy impact strength (+23°C) N / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 220 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 55 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 150 / * °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 190 / * °C ISO 306
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 3.2 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Volume resistivity 1E13 / 1E10 Ohm*m IEC 60093
Surface resistivity * / 1E12 Ohm IEC 60093
Comparative tracking index 600 / - - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 9 / * % Sim. to ISO 62
Humidity absorption 2.4 / * % Sim. to ISO 62
Density 1110 / - kg/m³ ISO 1183
Characteristics
Processing
Injection Molding
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Any information given on the chemical and physical characteristics of
our products, including technical advice on applications whether
verbally, in writing or by testing the product, is given to the best
of our knowledge, but without warranty. It does not exempt the buyer
from carrying out his own investigations and tests in order to
ascertain the products' specific suitability for the purpose intended.

The buyer is solely responsible for the application, utilisation and
processing of the products, and must observe the laws and government
regulations and the consequential rights of any third party. At all
times our Conditions of Sale apply.

The test values given are guide values, not binding minimum or maximum
figures, which have been determined on standardized test specimen and
can be affected by pigmentation, mold design and processing conditions.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991