CAMPUS® datasheet | Akulon® Ultraflow K-FKGS6


This datasheet of Akulon® Ultraflow K-FKGS6 from DSM Engineering Plastics is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Akulon® Ultraflow K-FKGS6 | PA6-GF30 FR(17) | DSM Engineering Plastics
Product Texts
30% Glass Reinforced, Heat Stabilized, Flame Retardant, High Flow

ISO 1043 PA6-GF30 FR(17)

Akulon® polyamide 6 and 66 resins
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 11500 / 7000 MPa ISO 527-1/-2
Stress at break 150 / 100 MPa ISO 527-1/-2
Strain at break 2.5 / 5 % ISO 527-1/-2
Charpy impact strength (+23°C) 60 / 60 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 60 / 60 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 13 / 15 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 12 / 12 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 220 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 205 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 215 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 20 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 110 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. V-0 / * class IEC 60695-11-10
Thickness tested 1.5 / * mm IEC 60695-11-10
UL recognition UL / * - -
Burning Behav. at thickness h V-0 / * class IEC 60695-11-10
Thickness tested 0.8 / * mm IEC 60695-11-10
UL recognition UL / * - -
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 3.5 / 10 - IEC 60250
Relative permittivity (1MHz) 3.4 / 4 - IEC 60250
Dissipation factor (100Hz) 60 / 3000 E-4 IEC 60250
Dissipation factor (1MHz) 120 / 700 E-4 IEC 60250
Volume resistivity 1E13 / 1E11 Ohm*m IEC 60093
Surface resistivity * / 1E14 Ohm IEC 60093
Comparative tracking index - / 425 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 4.5 / * % Sim. to ISO 62
Humidity absorption 1.3 / * % Sim. to ISO 62
Density 1590 / - kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1150 kg/m³ -
Thermal conductivity of melt 0.26 W/(m K) -
Spec. heat capacity melt 1900 J/(kg K) -
Eff. thermal diffusivity 1.20E-7 m²/s -
Diagrams
Stress-strain , Akulon® Ultraflow K-FKGS6, PA6-GF30 FR(17), DSM
Stress-strain , Akulon® Ultraflow K-FKGS6, PA6-GF30 FR(17), DSM
Secant modulus-strain , Akulon® Ultraflow K-FKGS6, PA6-GF30 FR(17), DSM
Secant modulus-strain , Akulon® Ultraflow K-FKGS6, PA6-GF30 FR(17), DSM
Specific volume-temperature (pvT) , Akulon® Ultraflow K-FKGS6, PA6-GF30 FR(17), DSM
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
Disclaimer
 All information supplied by or on behalf of DSM in relation to its
products, whether in the nature of data, recommendations or otherwise,
is supported by research and, in good faith, believed reliable, but DSM
assumes no liability and makes no warranties of any kind, express or
implied, including, but not limited to, those of title, merchantability,
fitness for a particular purpose or non-infringement or any warranty
arising from a course of dealing, usage, or trade practice whatsoever
in respect of application, processing or use made of the aforementioned
information or product. The user assumes all responsibility for the use
of all information provided and shall verify quality and other properties or
any consequence from the use of all such information.

Typical values are indicative only and are not to be construed as being
binding specifications.