This datasheet of Arnite® AV2 372 from DSM Engineering Plastics is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Arnite® AV2 372 | PET-GF35 | DSM Engineering Plastics
Product Texts
35% Glass Reinforced

ISO 1043 PET-GF35

Arnite® PBT and PET Polyesters
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 13000 MPa ISO 527-1/-2
Stress at break 190 MPa ISO 527-1/-2
Strain at break 2.5 % ISO 527-1/-2
Charpy impact strength (+23°C) 50 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 50 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 10 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 10 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 255 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 235 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 250 °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 25 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 40 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm IEC 60695-11-10
UL recognition UL - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
UL recognition UL - -
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.3 - IEC 60250
Relative permittivity (1MHz) 3.1 - IEC 60250
Dissipation factor (100Hz) 30 E-4 IEC 60250
Dissipation factor (1MHz) 130 E-4 IEC 60250
Volume resistivity >1E13 Ohm*m IEC 60093
Electric strength 34 kV/mm IEC 60243-1
Comparative tracking index 250 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.45 % Sim. to ISO 62
Humidity absorption 0.18 % Sim. to ISO 62
Density 1630 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1350 kg/m³ -
Thermal conductivity of melt 0.195 W/(m K) -
Spec. heat capacity melt 1670 J/(kg K) -
Eff. thermal diffusivity 8.67E-8 m²/s -
Diagrams
Viscosity-shear rate , Arnite® AV2 372, PET-GF35, DSM
Shearstress-shear rate , Arnite® AV2 372, PET-GF35, DSM
Dynamic Shear modulus-temperature , Arnite® AV2 372, PET-GF35, DSM
Stress-strain , Arnite® AV2 372, PET-GF35, DSM
Secant modulus-strain , Arnite® AV2 372, PET-GF35, DSM
Stress-strain (isochronous) 23°C, Arnite® AV2 372, PET-GF35, DSM
Creep modulus-time 23°C, Arnite® AV2 372, PET-GF35, DSM
Stress-strain (isochronous) 40°C, Arnite® AV2 372, PET-GF35, DSM
Specific volume-temperature (pvT) , Arnite® AV2 372, PET-GF35, DSM
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Regional Availability
Other text information
Injection molding
Disclaimer
 All information supplied by or on behalf of DSM in relation to its
products, whether in the nature of data, recommendations or otherwise,
is supported by research and, in good faith, believed reliable, but DSM
assumes no liability and makes no warranties of any kind, express or
implied, including, but not limited to, those of title, merchantability,
fitness for a particular purpose or non-infringement or any warranty
arising from a course of dealing, usage, or trade practice whatsoever
in respect of application, processing or use made of the aforementioned
information or product. The user assumes all responsibility for the use
of all information provided and shall verify quality and other properties or
any consequence from the use of all such information.

Typical values are indicative only and are not to be construed as being
binding specifications.