Arnite® T06 200 | PBT | DSM Engineering Plastics
Product Texts
| Rheological properties | Value | Unit | Test Standard |
| Melt volume-flow rate (MVR) | 22 | cm³/10min | ISO 1133 |
| Temperature | 250 | °C | ISO 1133 |
| Load | 2.16 | kg | ISO 1133 |
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 2700 | MPa | ISO 527-1/-2 |
| Yield stress | 55 | MPa | ISO 527-1/-2 |
| Yield strain | 3.5 | % | ISO 527-1/-2 |
| Nominal strain at break | >50 | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | N | kJ/m² | ISO 179/1eU |
| Charpy impact strength (-30°C) | N | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 5 | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | 5 | kJ/m² | ISO 179/1eA |
| Thermal properties | Value | Unit | Test Standard |
| Melting temperature (10°C/min) | 225 | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 55 | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 165 | °C | ISO 75-1/-2 |
| Coeff. of linear therm. expansion (parallel) | 90 | E-6/K | ISO 11359-1/-2 |
| Coeff. of linear therm. expansion (normal) | 90 | E-6/K | ISO 11359-1/-2 |
| Burning Behav. at 1.5 mm nom. thickn. | HB | class | IEC 60695-11-10 |
| Thickness tested | 1.5 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Burning Behav. at thickness h | HB | class | IEC 60695-11-10 |
| Thickness tested | 0.8 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Electrical properties | Value | Unit | Test Standard |
| Relative permittivity (100Hz) | 3.5 | - | IEC 60250 |
| Relative permittivity (1MHz) | 3.2 | - | IEC 60250 |
| Dissipation factor (100Hz) | 20 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | 200 | E-4 | IEC 60250 |
| Volume resistivity | >1E13 | Ohm*m | IEC 60093 |
| Electric strength | 27 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 600 | - | IEC 60112 |
| Other properties | Value | Unit | Test Standard |
| Water absorption | 0.45 | % | Sim. to ISO 62 |
| Humidity absorption | 0.18 | % | Sim. to ISO 62 |
| Density | 1300 | kg/m³ | ISO 1183 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Density of melt | 1040 | kg/m³ | - |
| Thermal conductivity of melt | 0.109 | W/(m K) | - |
| Spec. heat capacity melt | 2260 | J/(kg K) | - |
| Eff. thermal diffusivity | 4.65E-8 | m²/s | - |
Diagrams
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets
Regional Availability
Disclaimer
All information supplied by or on behalf of DSM in relation to its products, whether in the nature of data, recommendations or otherwise, is supported by research and, in good faith, believed reliable, but DSM assumes no liability and makes no warranties of any kind, express or implied, including, but not limited to, those of title, merchantability, fitness for a particular purpose or non-infringement or any warranty arising from a course of dealing, usage, or trade practice whatsoever in respect of application, processing or use made of the aforementioned information or product. The user assumes all responsibility for the use of all information provided and shall verify quality and other properties or any consequence from the use of all such information. Typical values are indicative only and are not to be construed as being binding specifications.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991