CAMPUS® datasheet | Arnitel® EL740


This datasheet of Arnitel® EL740 from DSM Engineering Plastics is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Arnitel® EL740 | TPC | DSM Engineering Plastics
Product Texts
72 Shore D, Injection Molding

ISO 18064 TPC-ET

Arnitel® copolyester elastomers
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 15 cm³/10min ISO 1133
Temperature 230 °C ISO 1133
Load 2.16 kg ISO 1133
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 1000 MPa ISO 527-1/-2
Yield stress 34 MPa ISO 527-1/-2
Yield strain 10 % ISO 527-1/-2
Nominal strain at break >50 % ISO 527-1/-2
Stress at 10% elongation 34.4 MPa ISO 527-1/-2
Stress at break TPE 38 MPa ISO 527-1/-2
Strain at break TPE 250 % ISO 527-1/-2
Charpy notched impact strength (+23°C) 10 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 6 kJ/m² ISO 179/1eA
Compression Set under constant strain (23°C) 20 % ISO 815
Compression Set under constant strain (70°C) 35 % ISO 815
Tear strength 260 kN/m ISO 34-1
Shore D hardness (15s) 72 - ISO 868
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 221 °C ISO 11357-1/-3
Temp. of deflection under load (0.45 MPa) 120 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 160 °C ISO 306
Coeff. of linear therm. expansion (parallel) 165 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 165 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.6 mm IEC 60695-11-10
UL recognition UL - -
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.7 - IEC 60250
Relative permittivity (1MHz) 3.3 - IEC 60250
Dissipation factor (1MHz) 300 E-4 IEC 60250
Volume resistivity 1E13 Ohm*m IEC 60093
Electric strength 23 kV/mm IEC 60243-1
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.6 % Sim. to ISO 62
Humidity absorption 0.15 % Sim. to ISO 62
Density 1290 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 950 kg/m³ -
Thermal conductivity of melt 0.1 W/(m K) -
Spec. heat capacity melt 1900 J/(kg K) -
Eff. thermal diffusivity 5.54E-8 m²/s -
Ejection temperature 160 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 240 °C ISO 294
Injection Molding, mold temperature 35 °C ISO 10724
Injection Molding, injection velocity 500 mm/s ISO 294
Diagrams
Viscosity-shear rate , Arnitel® EL740, TPC, DSM
Shearstress-shear rate , Arnitel® EL740, TPC, DSM
Dynamic Shear modulus-temperature , Arnitel® EL740, TPC, DSM
Specific volume-temperature (pvT) , Arnitel® EL740, TPC, DSM
Stress-Strain (TPE) , Arnitel® EL740, TPC, DSM
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
<font face="Arial" size="2">Injection Molding Recommendations
Disclaimer
 All information supplied by or on behalf of DSM in relation to its
products, whether in the nature of data, recommendations or otherwise,
is supported by research and, in good faith, believed reliable, but DSM
assumes no liability and makes no warranties of any kind, express or
implied, including, but not limited to, those of title, merchantability,
fitness for a particular purpose or non-infringement or any warranty
arising from a course of dealing, usage, or trade practice whatsoever
in respect of application, processing or use made of the aforementioned
information or product. The user assumes all responsibility for the use
of all information provided and shall verify quality and other properties or
any consequence from the use of all such information.

Typical values are indicative only and are not to be construed as being
binding specifications.