This datasheet of BERGAMID® B70GGK30 from PolyOne Engineered Materials Europe is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
glass fibre and glass bead, good surface finish
| Mechanical properties | dry / cond | Unit | Test Standard |
| Tensile Modulus | 4000 / 6500 | MPa | ISO 527-1/-2 |
| Stress at break | 60 / 110 | MPa | ISO 527-1/-2 |
| Strain at break | 5 / 3 | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | 85 / 60 | kJ/m² | ISO 179/1eU |
| Charpy impact strength (-30°C) | - / 50 | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 14 / 7 | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | - / 6 | kJ/m² | ISO 179/1eA |
| Thermal properties | dry / cond | Unit | Test Standard |
| Melting temperature (10°C/min) | 223 / * | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 190 / * | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 210 / * | °C | ISO 75-1/-2 |
| Burning Behav. at 1.5 mm nom. thickn. | HB / * | class | IEC 60695-11-10 |
| Thickness tested | 1.6 / * | mm | IEC 60695-11-10 |
| Burning Behav. at thickness h | HB / * | class | IEC 60695-11-10 |
| Thickness tested | 0.8 / * | mm | IEC 60695-11-10 |
| Electrical properties | dry / cond | Unit | Test Standard |
| Relative permittivity (1MHz) | 6.8 / 3.8 | - | IEC 60250 |
| Dissipation factor (1MHz) | 2400 / 270 | E-4 | IEC 60250 |
| Volume resistivity | 1E10 / 1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | * / 1E10 | Ohm | IEC 60093 |
| Comparative tracking index | 500 / - | - | IEC 60112 |
| Other properties | dry / cond | Unit | Test Standard |
| Water absorption | 6.7 / * | % | Sim. to ISO 62 |
| Humidity absorption | 2.1 / * | % | Sim. to ISO 62 |
| Density | - / 1350 | kg/m³ | ISO 1183 |
| Material specific properties | dry / cond | Unit | Test Standard |
| Viscosity number | 150 / * | cm³/g | ISO 307, 1157, 1628 |
| Test specimen production | Value | Unit | Test Standard |
| Injection Molding, melt temperature | 270 | °C | ISO 294 |
| Injection Molding, mold temperature | 80 | °C | ISO 10724 |
Max. Water Content 0,1%
Pre-Drying: 80°C 4 Hours
PROCESSING
Melt Temperature 270-290°C
Mould Temperature 80-90°C
PolyOnePolyOne Engineered Materials Europe
PolyOne Th.Bergmann GmbH
PolyOne Corporation makes no representations, guarantees or warranties of any kind with respect to the information contained in this document about its accuracy, suitability for particular applications ort he result obtained or obtainable using the information. Some of the information arises from laboratory work with small-case equipment which may not provide a reliable indication of performance or properties obtained or obtainable on larger-scale equipment. Processing conditions can cause material properties to shift from the values stated in data bases. PolyOne Corporation makes no guarantees or warranties respecting suitability of either PolyOne’s products or the information for your process or end-use application. You have the responsibility to conduct full-scale end-product performance testing to determine suitability in your application, and you assume all risks and liability arising from your use of the information and/or handling of any product. PolyOne Corporation makes no warranties, express or implied, including, but not limited to, implied warranties of merchantability and fitness for a particular purpose, either with respect to the information or products reflected by the information. These information shall not operate as permission, recommendation or inducement to practice any patented invention without permission of the patent owner.
Germany:
PolyOne Th.Bergmann GmbH
Adolf-Dambach-Strasse 2-4
D-76571 Gaggenau
Tel.: 07225 6802 0
Fax:07225 6802 10
France:
PolyOne Engineered Materials SA, FRANCE
20, Rue Salvador Allende, BP 105
42353 La Talaudière Cedex, France
Tel.: +33 (0) 477 47 64 00
Tel.:+33 (0) 477 57 13
Spain:
Pol. Ind. Valle del Cinca
22300 Barbastro, Spain
Tel.: +34 (0) 974 31 03 14
Fax.: +34 (0) 974 31 43 11
United Kingdom:
PolyOne Engineered Materials UL Ltd.
Newton Ayecliff
Durham DL5 6EA, UK
Tel.:+44 (0) 1325 30 08 48
Fax.:+44 (0) 1325 30 14 13
Turkey:
Tekno Polimer
103 Kücükcekmece
Istanbul, Turkey
Tel:+90 212 549 2256
Fax.:+90 212 549 2241
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991