  CELANEX 2404 MT | PBT | Ticona
Product Texts
Celanex 2404 MT Natural is an unreinforced PTFE filled PBT with
improved friction, sliding, and wear properties that complies with the
requirements of CFR 21 177.1660 of the Food and Drug Administration
(FDA) and is listed in the Drug Master File (DMF) 10047 (US) / 10033
(EU) and the Device Master File (MAF) 443 (US) / 1078 (EU).. 2404 MT
also complies with the corresponding EU and national registry
regulatory requirements. 2404 MT has displayed excellent
biocompatibility in tests corresponding to USP 23 class VI. Celanex
2404 MT contains no animal derived materials.
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 21 cm³/10min ISO 1133
Temperature 250 °C ISO 1133
Load 2.16 kg ISO 1133
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2600 MPa ISO 527-1/-2
Yield stress 56 MPa ISO 527-1/-2
Yield strain 7 % ISO 527-1/-2
Nominal strain at break 19 % ISO 527-1/-2
Charpy notched impact strength (+23°C) 3.3 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 225 °C ISO 11357-1/-3
Glass transition temperature (10°C/min) 60 °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 55 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 190 °C ISO 306
Electrical propertiesValueUnitTest Standard
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Density 1340 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Processing conditions acc. ISO 7790 - ISO ....-2
Injection Molding, melt temperature 243 °C ISO 294
Injection Molding, mold temperature 82 °C ISO 10724
Injection Molding, injection velocity 300 mm/s ISO 294
Injection Molding, pressure at hold 48 MPa ISO 294
Characteristics
Processing
Injection Molding
Regional Availability
Other text information
Injection molding
PREPROCESSING
To avoid hydrolytic degradation during processing, CELANEX resins have
to be dried to a moisture level equal to or less than 0.02%. Drying
should be done in a dehumidifying hopper dryer capable of dewpoints
<-30°F (-34°C) at 250°F (121°C) for 4 hours.

PROCESSING
Rear Temperature 450-470(230-240) deg F (deg C)
Center Temperature 460-480(235-250) deg F (deg C)
Front Temperature 470-500(240-260) deg F (deg C)
Nozzle Temper ature 480-500(250-260) deg F (deg C)
Melt Temperature 460-500(235-260) deg F (deg C)
Mold Temperature 150-200(65-93) deg F (deg C)
Back Pressure 0-50 psi
Screw Speed Medium
Injection Speed Fast

Injection speed, injection pressure and holding pressure have to be
optimized to the individual article geometry. To avoid material
degradation during processing low back pressure and minimum screw speed
have to be used. Ov erheating of the material has to be avoided, in
particular for flame retardant grades. Up to 25% clean and dry regrind
may be used.

POSTPROCESSING
Disclaimer
NOTICE TO USERS: Values shown are based on testing
of laboratory test specimens and represent data that fall
within the standard range of properties for natural material.
These values alone do not represent a sufficient basis for
any part design and are not intended for use in
establishing maximum, minimum, or ranges of values for
specification purposes. Colorants or other additives may
cause significant variations in data values.

Properties of molded parts can be influenced by a wide
variety of factors including, but not limited to, material
selection, additives, part design, processing conditions and
environmental exposure. Any determination of the
suitability of a particular material and part design for any
use contemplated by the users and the manner of such
use is the sole responsibility of the users, who must assure
themselves that the material as subsequently processed
meets the needs of their particular product or use.

To the best of our knowledge, the information contained in
this publication is accurate; however, we do not assume
any liability whatsoever for the accuracy and completeness
of such information. The information contained in this
publication should not be construed as a promise or
guarantee of specific properties of our products. It is the
sole responsibility of the users to investigate whether any
existing patents are infringed by the use of the materials
mentioned in this publication.

Moreover, there is a need to reduce human exposure to
many materials to the lowest practical limits in view of
possible adverse effects. To the extent that any hazards
may have been mentioned in this publication, we neither
suggest nor guarantee that such hazards are the only ones
which exist. We recommend that persons intending to rely
on any recommendation or to use any equipment,
processing technique, or material mentioned in this
publication should satisfy themselves that they can meet
all applicable safety and health standards.

We strongly recommend that users seek and adhere to the
manufacturer's current instructions for handling each
material they use, and to entrust the handling of such
material to adequately trained personnel only. Please call
the telephone numbers listed for additional technical
information. Call Customer Services for the appropriate
Materials Safety Data Sheets (MSDS) before attempting to
process our products.

The products mentioned herein are not intended for use in
medical or dental implants.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991