  CELANEX 3216 | PBT-GF15 | Ticona
Product Texts
Celanex 3216 is a non-exuding (UL and CSA approved V-0 at 1/32 inch and
5V at 1/8 inch ),15% fiberglass reinforced polybutylene terephthalate
which has an excellent balance of mechanical properties and
processability. It is well suited for electrical connector applications
where its UL approved 50% regrind use capability allows maximum use of
purchased product.
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 9 cm³/10min ISO 1133
Temperature 250 °C ISO 1133
Load 2.16 kg ISO 1133
Molding shrinkage (normal) 1.1 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 6700 MPa ISO 527-1/-2
Stress at break 100 MPa ISO 527-1/-2
Strain at break 3 % ISO 527-1/-2
Charpy impact strength (+23°C) 28 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 28 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 6 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 225 °C ISO 11357-1/-3
Glass transition temperature (10°C/min) 60 °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 200 °C ISO 75-1/-2
Temp. of deflection under load (8.00 MPa) 95 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 206 °C ISO 306
Coeff. of linear therm. expansion (parallel) 36 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 100 E-6/K ISO 11359-1/-2
Burning Behav. at thickness h V-0 class IEC 60695-11-10
Thickness tested 0.4 mm IEC 60695-11-10
Burning Behav. 5V at thickness h 5VA class IEC 60695-11-20
Thickness tested 3.0 mm IEC 60695-11-20
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.7 - IEC 60250
Relative permittivity (1MHz) 3.5 - IEC 60250
Dissipation factor (100Hz) 33 E-4 IEC 60250
Dissipation factor (1MHz) 160 E-4 IEC 60250
Volume resistivity 1E13 Ohm*m IEC 60093
Surface resistivity 1E15 Ohm IEC 60093
Electric strength 30 kV/mm IEC 60243-1
Comparative tracking index 250 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.4 % Sim. to ISO 62
Humidity absorption 0.17 % Sim. to ISO 62
Density 1540 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Processing conditions acc. ISO 7790 - ISO ....-2
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 82 °C ISO 10724
Injection Molding, injection velocity 300 mm/s ISO 294
Injection Molding, pressure at hold 48 MPa ISO 294
Diagrams
Viscosity-shear rate , CELANEX 3216, PBT-GF15, Ticona
Shearstress-shear rate , CELANEX 3216, PBT-GF15, Ticona
Stress-strain , CELANEX 3216, PBT-GF15, Ticona
Secant modulus-strain , CELANEX 3216, PBT-GF15, Ticona
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants
Regional Availability
Other text information
Injection molding
PREPROCESSING
To avoid hydrolytic degradation during processing, CELANEX resins have
to be dried to a moisture level equal to or less than 0.02%. Drying
should be done in a dehumidifying hopper dryer capable of dewpoints
<-30°F (-34°C) at 250°F (121°C) for 4 hours..

PROCESSING
Rear Temperature 450-470(230-240) deg F (deg C)
Center Temperature 460-480(235-250) deg F (deg C)
Front Temperature 470-490(240-255) deg F (deg C)
Nozzle Tempe rature 480-490(250-255) deg F (deg C)
Melt Temperature 460-490(235-255) deg F (deg C)
Mold Temperature 150-200(65-93) deg F (deg C)
Back Pressure 0-50 psi
Screw Speed Medium
Injection Speed Fast

Injection speed, injection pressure and holding pressure have to be
optimized to the individual article geometry. To avoid material
degradation during processing low back pressure and minimum screw speed
have to be used. O verheating of the material has to be avoided, in
particular for flame retardant grades. Up to 50% clean and dry regrind
may be used for the '16 series' flame retardant grades.

POSTPROCESSING
Disclaimer
NOTICE TO USERS: Values shown are based on testing
of laboratory test specimens and represent data that fall
within the standard range of properties for natural material.
These values alone do not represent a sufficient basis for
any part design and are not intended for use in
establishing maximum, minimum, or ranges of values for
specification purposes. Colorants or other additives may
cause significant variations in data values.

Properties of molded parts can be influenced by a wide
variety of factors including, but not limited to, material
selection, additives, part design, processing conditions and
environmental exposure. Any determination of the
suitability of a particular material and part design for any
use contemplated by the users and the manner of such
use is the sole responsibility of the users, who must assure
themselves that the material as subsequently processed
meets the needs of their particular product or use.

To the best of our knowledge, the information contained in
this publication is accurate; however, we do not assume
any liability whatsoever for the accuracy and completeness
of such information. The information contained in this
publication should not be construed as a promise or
guarantee of specific properties of our products. It is the
sole responsibility of the users to investigate whether any
existing patents are infringed by the use of the materials
mentioned in this publication.

Moreover, there is a need to reduce human exposure to
many materials to the lowest practical limits in view of
possible adverse effects. To the extent that any hazards
may have been mentioned in this publication, we neither
suggest nor guarantee that such hazards are the only ones
which exist. We recommend that persons intending to rely
on any recommendation or to use any equipment,
processing technique, or material mentioned in this
publication should satisfy themselves that they can meet
all applicable safety and health standards.

We strongly recommend that users seek and adhere to the
manufacturer's current instructions for handling each
material they use, and to entrust the handling of such
material to adequately trained personnel only. Please call
the telephone numbers listed for additional technical
information. Call Customer Services for the appropriate
Materials Safety Data Sheets (MSDS) before attempting to
process our products.

The products mentioned herein are not intended for use in
medical or dental implants.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991