CELCON LU-02 | POM | Ticona
Product Texts
Celcon® acetal copolymer grade LU-02 is UV stabilized material
displaying a reduced gloss over standard UV acetal grades.
displaying a reduced gloss over standard UV acetal grades.
| Rheological properties | Value | Unit | Test Standard |
| Melt volume-flow rate (MVR) | 20 | cm³/10min | ISO 1133 |
| Temperature | 190 | °C | ISO 1133 |
| Load | 2.16 | kg | ISO 1133 |
| Molding shrinkage (parallel) | 1.9 | % | ISO 294-4, 2577 |
| Molding shrinkage (normal) | 1.6 | % | ISO 294-4, 2577 |
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 2530 | MPa | ISO 527-1/-2 |
| Yield stress | 56 | MPa | ISO 527-1/-2 |
| Yield strain | 9 | % | ISO 527-1/-2 |
| Nominal strain at break | 11 | % | ISO 527-1/-2 |
| Charpy notched impact strength (+23°C) | 3.7 | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | 3.7 | kJ/m² | ISO 179/1eA |
| Thermal properties | Value | Unit | Test Standard |
| Melting temperature (10°C/min) | 167 | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 90 | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 161 | °C | ISO 306 |
| Other properties | Value | Unit | Test Standard |
| Density | 1390 | kg/m³ | ISO 1183 |
| Test specimen production | Value | Unit | Test Standard |
| Processing conditions acc. ISO | 9990 | - | ISO ....-2 |
| Injection Molding, melt temperature | 205 | °C | ISO 294 |
| Injection Molding, mold temperature | 90 | °C | ISO 10724 |
| Injection Molding, injection velocity | 200 | mm/s | ISO 294 |
| Injection Molding, pressure at hold | 86 | MPa | ISO 294 |
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Drying is recommended for low gloss grades of Celcon® and Hostaform®
acetal copolymers. Excessive moisture can lead to splay (silver
streaking) in molded parts. For better uniformity in molding especially
when using regrind or material that has been stored in containers open
to the atmosphere, recommended drying conditions are 80 C (180 F) for
3hours. Desiccant hopper dryers are not required. Maximum water content
= 0.35%
PROCESSING
Standard reciprocating screw injection molding machines with a high
compression screw (minimum 3:1 and preferably 4:1) and low back
pressure (0.35 Mpa/50 PSI) are favored. Using a low compression screw
(I.E. general purpose 2:1 compression ratio) can result in unmelted
particles and poor melt homogeneity. Using a high back pressure to make
up for a low compression ratio may lead to excessive shear heating and
deterioration of the material.
Use a slow i njection speed until material passes through the gate.
Melt Temperature: Preferred range 180-195 C (~356-~383 F). Melt
temperature should never exceed 230 C (450 F).
Mold Surface Temperature: Preferred range 80-105 C especially with
wall thickness less than 1.5 mm (0.060 in.). May require mold
temperature as high as 120 C (250 F) to reproduce mold surface or to
assure minimal molded in stress. In general, mold surface temperatures
lower than 82 C ( 180 F) may produce a hazy surface or a surface with
flow lines, pits and other included defects.
POSTPROCESSING
Postprocessing conditioning and moisturizing are not required. It may
be necessary to fixture large or complicated parts with varying wall
thickness to prevent warpage while cooling to ambient temperature.
Drying is recommended for low gloss grades of Celcon® and Hostaform®
acetal copolymers. Excessive moisture can lead to splay (silver
streaking) in molded parts. For better uniformity in molding especially
when using regrind or material that has been stored in containers open
to the atmosphere, recommended drying conditions are 80 C (180 F) for
3hours. Desiccant hopper dryers are not required. Maximum water content
= 0.35%
PROCESSING
Standard reciprocating screw injection molding machines with a high
compression screw (minimum 3:1 and preferably 4:1) and low back
pressure (0.35 Mpa/50 PSI) are favored. Using a low compression screw
(I.E. general purpose 2:1 compression ratio) can result in unmelted
particles and poor melt homogeneity. Using a high back pressure to make
up for a low compression ratio may lead to excessive shear heating and
deterioration of the material.
Use a slow i njection speed until material passes through the gate.
Melt Temperature: Preferred range 180-195 C (~356-~383 F). Melt
temperature should never exceed 230 C (450 F).
Mold Surface Temperature: Preferred range 80-105 C especially with
wall thickness less than 1.5 mm (0.060 in.). May require mold
temperature as high as 120 C (250 F) to reproduce mold surface or to
assure minimal molded in stress. In general, mold surface temperatures
lower than 82 C ( 180 F) may produce a hazy surface or a surface with
flow lines, pits and other included defects.
POSTPROCESSING
Postprocessing conditioning and moisturizing are not required. It may
be necessary to fixture large or complicated parts with varying wall
thickness to prevent warpage while cooling to ambient temperature.
Disclaimer
NOTICE TO USERS: Values shown are based on testing of laboratory test specimens and represent data that fall within the standard range of properties for natural material. These values alone do not represent a sufficient basis for any part design and are not intended for use in establishing maximum, minimum, or ranges of values for specification purposes. Colorants or other additives may cause significant variations in data values. Properties of molded parts can be influenced by a wide variety of factors including, but not limited to, material selection, additives, part design, processing conditions and environmental exposure. Any determination of the suitability of a particular material and part design for any use contemplated by the users and the manner of such use is the sole responsibility of the users, who must assure themselves that the material as subsequently processed meets the needs of their particular product or use. To the best of our knowledge, the information contained in this publication is accurate; however, we do not assume any liability whatsoever for the accuracy and completeness of such information. The information contained in this publication should not be construed as a promise or guarantee of specific properties of our products. It is the sole responsibility of the users to investigate whether any existing patents are infringed by the use of the materials mentioned in this publication. Moreover, there is a need to reduce human exposure to many materials to the lowest practical limits in view of possible adverse effects. To the extent that any hazards may have been mentioned in this publication, we neither suggest nor guarantee that such hazards are the only ones which exist. We recommend that persons intending to rely on any recommendation or to use any equipment, processing technique, or material mentioned in this publication should satisfy themselves that they can meet all applicable safety and health standards. We strongly recommend that users seek and adhere to the manufacturer's current instructions for handling each material they use, and to entrust the handling of such material to adequately trained personnel only. Please call the telephone numbers listed for additional technical information. Call Customer Services for the appropriate Materials Safety Data Sheets (MSDS) before attempting to process our products. The products mentioned herein are not intended for use in medical or dental implants.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991