View list of
  • All Ticona grades
  • All POM grades
  • All grades beginning with C

CAMPUS® datasheet | CELCON M90


This datasheet of CELCON M90 from Ticona is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  CELCON M90 | POM | Ticona
Product Texts
Celcon acetal copolymer grade M90™ is a medium viscosity polymer
providing optimum performance in general purpose injection molding and
extrusion of thin walled tubing and thin gauge film. This grade
provides overall excellent performance in many applications.

Chemical abbreviation according to ISO 1043-1: POM

Please also see Hostaform® C 9021.
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 8 cm³/10min ISO 1133
Temperature 190 °C ISO 1133
Load 2.16 kg ISO 1133
Molding shrinkage (parallel) 2.0 % ISO 294-4, 2577
Molding shrinkage (normal) 1.9 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2760 MPa ISO 527-1/-2
Tensile creep modulus (1h) 2450 MPa ISO 899-1
Tensile creep modulus (1000h) 1350 MPa ISO 899-1
Charpy impact strength (+23°C) 188 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 181 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 6 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 165 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 101 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 158 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 161 °C ISO 306
Coeff. of linear therm. expansion (parallel) 120 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 120 E-6/K ISO 11359-1/-2
Electrical propertiesValueUnitTest Standard
Volume resistivity 8E12 Ohm*m IEC 60093
Surface resistivity >1E15 Ohm IEC 60093
Other propertiesValueUnitTest Standard
Water absorption 0.75 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1410 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1200 kg/m³ -
Thermal conductivity of melt 0.155 W/(m K) -
Spec. heat capacity melt 2210 J/(kg K) -
Eff. thermal diffusivity 4.85E-8 m²/s -
Ejection temperature 165 °C -
Test specimen productionValueUnitTest Standard
Processing conditions acc. ISO 9990 - ISO ....-2
Injection Molding, melt temperature 205 °C ISO 294
Injection Molding, mold temperature 90 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Injection Molding, pressure at hold 86 MPa ISO 294
Diagrams
Stress-strain , CELCON M90, POM, Ticona
Secant modulus-strain , CELCON M90, POM, Ticona
Stress-strain (isochronous) 23°C, CELCON M90, POM, Ticona
Creep modulus-time 23°C, CELCON M90, POM, Ticona
Stress-strain (isochronous) 40°C, CELCON M90, POM, Ticona
Creep modulus-time 40°C, CELCON M90, POM, Ticona
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Sheet Extrusion, Other Extrusion, Blow Molding, Calandering
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Drying is generally not required because Celcon® and Hostaform® acetal
copolymers are not hydroscopic nor are they degraded by moisture during
processing. Excessive moisture can lead to splay (silver streaking) in
molded parts. For better uniformity in molding especially when using
regrind or material that has been stored in containers open to the
atmosphere, recommended drying conditions are 80 C (180 F) for 3hours.
Desiccant hopper dryers are not required. Maximum water content = 0.35%

PROCESSING
Standard reciprocating screw injection molding machines with a high
compression screw (minimum 3:1 and preferably 4:1) and low back
pressure (0.35 Mpa/50 PSI) are favored. Using a low compression screw
(I.E. general purpose 2:1 compression ratio) can result in unmelted
particles and poor melt homogeneity. Using a high back pressure to make
up for a low compression ratio may lead to excessive shear he ating and
deterioration of the material.

Melt Temperature: Preferred range 182-199 C (360-390 F). Melt
temperature should never exceed 230 C (450 F).

Mold Surface Temperature: Preferred range 82-93 C (180-200 F)
especially with wall thickness less than 1.5 mm (0.060 in.). May
require mold temperature as high as 120 C (250 F) to reproduce mold
surface or to assure minimal molded in stress. Wall thickness greater
than 3mm (1/8 in.) may use a coole r (65 C/150 F) mold surface
temperature and wall thickness over 6mm (1/4 in.) may use a cold mold
surface down to 25 C (80 F). In general, mold surface temperatures
lower than 82 C (180 F) may hinder weld line formation and produce a
hazy surface or a surface with flow lines, pits and other included
defects that can hinder part performance.

POSTPROCESSING
Postprocessing conditioning and moisturizing are not required. It may
be necessary to fixture large or complicated parts with varying wall
thickness to prevent warpage while cooling to ambient temperature.
Film extrusion
PREPROCESSING
Drying is generally not required because Celcon materials are not
hydroscopic nor are they degraded by moisture during processing.
Excessive moisture can cause surface defects on the extruded film. For
better uniformity especially when using regrind or material that has
been stored in containers open to the atmosphere, recommended drying
conditions are 3 Hrs. at 80 C (180 F). Desiccant hopper dryers are not
required. Max. moisture content = 0. 35%.

PROCESSING
Standard extruders with a length to diameter ratio of at least 20:1 are
recommended. The screw should be a high compression ratio of at least
3:1 and preferably 4:1 to assure good melting and melt homogeneity. The
design should be approximately 35% each for feed and metering sections
with the remaining 30% as the transition zone.

Melt temperature: 160-220 C (320-430 F)

POSTPROCESSING
Postprocessing conditioning or moistur izing is not required.
Other extrusion
PREPROCESSING
Drying is generally not required because Celcon materials are not
hydroscopic nor are they degraded by moisture during processing.
Excessive moisture can cause surface defects. For better uniformity
especially when using regrind or material that has been stored in
containers open to the atmosphere, recommended drying is 3 hours at 80
C (180 F). Desiccant hopper dryers are not required. Max. moisture
content = 0.35%

PROCESSING
Stan dard extruders with a length to diameter ratio of at least 20:1 are
recommended. The screw should be a high compression ratio of at least
3:1 and preferably 4:1 to assure good melting and uniform melt
homogeneity. The design should be approximately 35% each for the feed
and metering sections with the remaining 30% as transition zone.

Melt temperature 180-220 C (355-430F)

POSTPROCESSING
Postprocessing conditioning or moisturizing are not required. For thick
walled sections (>3mm or 1/8 in.), annealing is recommended to reduce
internal stresses.

Annealing temperature: 130-140 C (265-285 F)

Annealing time: 10 min/mm thickness
Profile extrusion
PREPROCESSING
Drying is generally not required because Celcon materials are not
hydroscopic nor are they degraded by moisture during processing.
Excessive moisture can cause surface defects on the extrusion. For
better uniformity especially when using regrind or material that has
been stored in containers open to the atmosphere, recommended drying
conditions are 3 Hrs. at 80 C (180 F). Desiccant hopper dryers are not
required. Max. moisture content = 0.035% .

PROCESSING
Standard extruders with a length to diameter ratio of at least 20:1 are
recommended. The screw should be a high compression ratio of at least
3:1 and preferably 4:1 to assure good melting and melt homogeneity. The
design should be approximately 35% each for feed and metering sections
with the remaining 30% as the transition zone.

Melt temperature: 180-220 C (360-430 F).

POSTPROCESSING
Postprocessing or moisturizing is not re quired. For thick walled
extrusions (>3 mm or 1/8 in.), annealing is recommended to reduce
internal stresses.

Annealing temperature: 130-140 C (265-285 F)
Annealing time: 10 min/mm thickness
Sheet extrusion
PREPROCESSING
Drying is generally not required because Celcon materials are not
hydroscopic nor are they degraded by moisture during processing.
Excessive moisture can lead to surface defects. For better uniformity
in sheet extrusion especially when using regrind or material that has
been stored in containers open to the atmosphere, recommended drying is
3 hours at 80 C (180 F). Desiccant hopper dryers are not required. Max.
water content = 0.35%.

PROCESSING
Standard extruders with a length to diameter ratio of at least 20:1 are
recommended. The screw should be a high compression ratio (at least 3:1
and preferably 4:1) to assure good melting and uniform melt
homogeneity. The screw design should be approximately 35% each for the
feed and metering sections with the remaining 30% as the transition
zone.

Melt temperature 180-190 C (355-375 F).

POSTPROCESSING
Postprocessing conditioning or moisturizing is not required. For thick
walled sections (>3mm or 1/8 in.), annealing is recommended to reduce
internal stresses.

Annealing temperature: 130-140 C (265-285 F)

Annealing time: 10 min/mm wall thickness
Blow molding
PREPROCESSING
Consult product information services.

PROCESSING
Consult product information services.

POSTPROCESSING
Consult product information services.
Calandering
PREPROCESSING
Consult product information services.

PROCESSING
Consult product information services.

POSTPROCESSING
Consult product information services.
Compression molding
PREPROCESSING
Consult product information services.

PROCESSING
Consult product information services.

POSTPROCESSING
Consult product information services.
Disclaimer
NOTICE TO USERS: Values shown are based on testing
of laboratory test specimens and represent data that fall
within the standard range of properties for natural material.
These values alone do not represent a sufficient basis for
any part design and are not intended for use in
establishing maximum, minimum, or ranges of values for
specification purposes. Colorants or other additives may
cause significant variations in data values.

Properties of molded parts can be influenced by a wide
variety of factors including, but not limited to, material
selection, additives, part design, processing conditions and
environmental exposure. Any determination of the
suitability of a particular material and part design for any
use contemplated by the users and the manner of such
use is the sole responsibility of the users, who must assure
themselves that the material as subsequently processed
meets the needs of their particular product or use.

To the best of our knowledge, the information contained in
this publication is accurate; however, we do not assume
any liability whatsoever for the accuracy and completeness
of such information. The information contained in this
publication should not be construed as a promise or
guarantee of specific properties of our products. It is the
sole responsibility of the users to investigate whether any
existing patents are infringed by the use of the materials
mentioned in this publication.

Moreover, there is a need to reduce human exposure to
many materials to the lowest practical limits in view of
possible adverse effects. To the extent that any hazards
may have been mentioned in this publication, we neither
suggest nor guarantee that such hazards are the only ones
which exist. We recommend that persons intending to rely
on any recommendation or to use any equipment,
processing technique, or material mentioned in this
publication should satisfy themselves that they can meet
all applicable safety and health standards.

We strongly recommend that users seek and adhere to the
manufacturer's current instructions for handling each
material they use, and to entrust the handling of such
material to adequately trained personnel only. Please call
the telephone numbers listed for additional technical
information. Call Customer Services for the appropriate
Materials Safety Data Sheets (MSDS) before attempting to
process our products.

The products mentioned herein are not intended for use in
medical or dental implants.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991