View list of
  • All Ticona grades
  • All PA666 grades
  • All grades beginning with C

CAMPUS® datasheet | CELSTRAN PA66-GF50-0111P1011


This datasheet of CELSTRAN PA66-GF50-0111P1011 from Ticona is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  CELSTRAN PA66-GF50-0111P10/11 | PA666-GF50 | Ticona
Product Texts
Material code according to ISO 1043-1: PA66

Nylon 66/6 Copolymer reinforced by 50 weight percent long glass
fibers. The pellets are cylindrical and normally as well as the
embedded fibers 10 mm long.

Parts molded of CELSTRAN have outstanding mechanical properties such
as high strength and stiffness combined with high heat deflection.
The notched impact strength is increased at elevated and low
temperatures due to the fiber skeleton built in the parts. The long
fiber reinforcement reduces creep significantly.

The very isotropic shrinkage in the molded parts minimizes the
warpage.

Complex parts can be manufactured with high reproducibility by
injection molding.

Can be used for substituting die cast metal with the advantage of
Weight reduction, no corrosion problems, no post treatment.
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 16500 / 11600 MPa ISO 527-1/-2
Stress at break 260 / 180 MPa ISO 527-1/-2
Strain at break 2.2 / 2.5 % ISO 527-1/-2
Charpy impact strength (+23°C) 100 / 50 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 80 / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 40 / 36 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 42 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 240 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 235 / * °C ISO 75-1/-2
Temp. of deflection under load (8.00 MPa) 220 / * °C ISO 75-1/-2
Other propertiesdry / condUnitTest Standard
Humidity absorption 1 / * % Sim. to ISO 62
Density 1570 / 1570 kg/m³ ISO 1183
Characteristics
Regional Availability
Other text information
Injection molding
PREPROCESSING

It is recommended to dry in a dehumidifying dryer: 4 hours at 80 °C




PROCESSING

During the processing of CELSTRAN it is important to watch and
control melt shear, for excessive shear reduces fiber length and
mechanical performance as well.

Processing recommendation:

- Conventional 3 zone screw, screw diameter minimum 40 mm
- Design flow channels for low melt shear
- Back pressure and screw rotation to realize a continous
plastification performance and thus a homogeneous melt.
- Apply higher temperature settings than for short fiber compounds

Melt temperature (in the srew anteroom) 310-325 °C
Mold surface temperature 90-120 °C



POSTPROCESSING
Disclaimer
NOTICE TO USERS: Values shown are based on testing
of laboratory test specimens and represent data that fall
within the standard range of properties for natural material.
These values alone do not represent a sufficient basis for
any part design and are not intended for use in
establishing maximum, minimum, or ranges of values for
specification purposes. Colorants or other additives may
cause significant variations in data values.

Properties of molded parts can be influenced by a wide
variety of factors including, but not limited to, material
selection, additives, part design, processing conditions and
environmental exposure. Any determination of the
suitability of a particular material and part design for any
use contemplated by the users and the manner of such
use is the sole responsibility of the users, who must assure
themselves that the material as subsequently processed
meets the needs of their particular product or use.

To the best of our knowledge, the information contained in
this publication is accurate; however, we do not assume
any liability whatsoever for the accuracy and completeness
of such information. The information contained in this
publication should not be construed as a promise or
guarantee of specific properties of our products. It is the
sole responsibility of the users to investigate whether any
existing patents are infringed by the use of the materials
mentioned in this publication.

Moreover, there is a need to reduce human exposure to
many materials to the lowest practical limits in view of
possible adverse effects. To the extent that any hazards
may have been mentioned in this publication, we neither
suggest nor guarantee that such hazards are the only ones
which exist. We recommend that persons intending to rely
on any recommendation or to use any equipment,
processing technique, or material mentioned in this
publication should satisfy themselves that they can meet
all applicable safety and health standards.

We strongly recommend that users seek and adhere to the
manufacturer's current instructions for handling each
material they use, and to entrust the handling of such
material to adequately trained personnel only. Please call
the telephone numbers listed for additional technical
information. Call Customer Services for the appropriate
Materials Safety Data Sheets (MSDS) before attempting to
process our products.

The products mentioned herein are not intended for use in
medical or dental implants.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991