CAMPUS® datasheet | Crastin® S610SF BK851


This datasheet of Crastin® S610SF BK851 from DuPont Engineering Polymers is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Crastin® S610SF BK851 | PBT | DuPont Engineering Polymers
Rheological propertiesValueUnitTest Standard
Molding shrinkage (parallel) 1.7 % ISO 294-4, 2577
Molding shrinkage (normal) 1.6 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2600 MPa ISO 527-1/-2
Yield stress 60 MPa ISO 527-1/-2
Yield strain 10 % ISO 527-1/-2
Nominal strain at break 13 % ISO 527-1/-2
Charpy notched impact strength (+23°C) 4 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 3.5 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 224 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 54 °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 130 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 130 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm IEC 60695-11-10
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
Oxygen index 22 % ISO 4589-1/-2
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.8 - IEC 60250
Relative permittivity (1MHz) 3.2 - IEC 60250
Dissipation factor (100Hz) 20 E-4 IEC 60250
Dissipation factor (1MHz) 200 E-4 IEC 60250
Volume resistivity >1E13 Ohm*m IEC 60093
Surface resistivity 1E12 Ohm IEC 60093
Electric strength 26 kV/mm IEC 60243-1
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.4 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1320 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1110 kg/m³ -
Thermal conductivity of melt 0.21 W/(m K) -
Spec. heat capacity melt 2110 J/(kg K) -
Ejection temperature 160 °C -
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Regional Availability
Disclaimer

E.I. du Pont de Nemours and Company is pleased to provide information about its products with the CAMPUS electronic database.

The information provided is gratis and DuPont assumes no obligation or liability for any advice furnished or for any results obtained with respect to this information.

All such advice is given and accepted at the risk of the buyer. The disclosure of information herein is not an express or implied license to operate under any patent of DuPont or others.

DuPont warrants that the use or sale of any material which is described herein and is offered for sale by DuPont does not infringe any patent covering the material itself, but does not warrant against infringement by reason of the use thereof in combination with other materials or the operation of any process.

Unless otherwise noted, the property values are for natural color (NC010) resins only. Colorants or other additives may alter some or all of the properties.
The data listed herein fall within the normal range of product properties and they should not be used to establish specification limits nor used alone as the basis of design.

Material Safety Data Sheets (SDSs) can be obtained from local sales offices.

Products listed herein should not be used in medical applications involving permanent implantation in the human body or contact with internal body fluids or tissues unless the material has been provided from DuPont under a written contract that is consistent with DuPont policy regarding medical applications and expressly acknowledges the contemplated use.

For further information, please contact your DuPont representative.

You may also request a copy of DuPont policy regarding medical applications H-50103-2 and DuPont caution regarding medical applications H-50102-2.

Products listed herein may from time to time be modified or removed.
Please call your local sales office to determine current availability.