View list of
CAMPUS® datasheet | Delrin® FG400XRD NC010
This datasheet of Delrin® FG400XRD NC010 from DuPont Engineering Polymers is provided by the international plastics database CAMPUS.
Delrin® FG400XRD NC010 | POM-MD25 | DuPont Engineering Polymers
Product Texts
Common features of Delrin® acetal resin include mechanical and physical properties such as high mechanical strength and rigidity, excellent fatigue and impact resistance, as well as resistance to moisture, gasoline, lubricants, solvents and many other neutral chemicals. Delrin® acetal resins also have excellent dimensional stability and good electrical insulating characteristics. They are naturally resilient, self-lubricating and available in a variety of colours and speciality grades.
The good melt stability of Delrin® acetal resin normally enables the recycling of properly handled production waste. If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-17 kJ/g of base polymer) in appropriately equipped installations. For disposal, local regulations have to be observed.
Delrin® acetal resin typically is used in demanding applications in the automotive, domestic appliances, sports, industrial engineering, electronics and consumer goods industries.
Delrin® FG400XRD is a filled, medium viscosity acetal copopolymer for injection molding. It is detected in X-ray detectors and is specifically suitable for the food industry.
| Rheological properties | Value | Unit | Test Standard |
| Melt volume-flow rate, MVR | 8 | cm³/10min | ISO 1133 |
| Temperature | 190 | °C | ISO 1133 |
| Load | 2.16 | kg | ISO 1133 |
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 3200 | MPa | ISO 527-1/-2 |
| Yield stress | 51 | MPa | ISO 527-1/-2 |
| Yield strain | 7 | % | ISO 527-1/-2 |
| Nominal strain at break | 15 | % | ISO 527-1/-2 |
| Charpy impact strength, +23°C | 80 | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength, +23°C | 4 | kJ/m² | ISO 179/1eA |
| Thermal properties | Value | Unit | Test Standard |
| Melting temperature, 10°C/min | 168 | °C | ISO 11357-1/-3 |
| Burning Behav. at 1.5 mm nom. thickn. | HB | class | IEC 60695-11-10 |
| Thickness tested | 1.5 | mm | IEC 60695-11-10 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Density of melt | 1420 | kg/m³ | - |
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Drying temperature = 80°C
Drying time, dehumidified dryer = 2-4 h
Processing moisture content = <0.2 %
PROCESSING
Melt temperature optimum = 205°C
Melt temperature range = 200-210°C
Mold temperature optimum = 90°C
Mold temperature range = 80-100°C
Hold pressure range = 80-100 MPa
Hold pressure time = 8-10 s/mm
Moulding guide
Drying temperature = 80°C
Drying time, dehumidified dryer = 2-4 h
Processing moisture content = <0.2 %
PROCESSING
Melt temperature optimum = 205°C
Melt temperature range = 200-210°C
Mold temperature optimum = 90°C
Mold temperature range = 80-100°C
Hold pressure range = 80-100 MPa
Hold pressure time = 8-10 s/mm
Moulding guide
Disclaimer
All data provided according to ISO 10350 for single points and ISO 11403 for multipoints.
Contact DuPont for Material Safety Data Sheet, general guides and/or additional information about ventilation, handling, purging, drying, etc.
Test temperatures are 23°C unless otherwise stated.
The DuPont Oval Logo, DuPont™, The miracles of science™ and ® are trademarks or registered trademarks of DuPont Company.
Copyright© 2011 E.I. du Pont de Nemours and Company. All Rights Reserved.
The information provided in this data sheet corresponds to our knowledge on the subject at the date of its publication.
This information may be subject to revision as new knowledge and experience becomes available.
The data provided fall within the normal range of product properties and relate only to the specific material designated; these data may not be
valid for such material used in combination with any other materials, additives or pigments or in any process, unless expressly indicated otherwise.
The data provided should not be used to establish specification limits or used alone as the basis of design; they are not intended to substitute
for any testing you may need to conduct to determine for yourself the suitability of a specific material for your particular purposes.
Since DuPont cannot anticipate all variations in actual end-use conditions DuPont makes no warranties and assumes no liability in connection
with any use of this information.
Nothing in this publication is to be considered as a license to operate under or a recommendation to infringe any patent rights.
DuPont advises you to seek independent counsel for a freedom to practice opinion on the intended application or end-use of our products.
CAUTION: DO NOT USE DUPONT MATERIALS IN MEDICAL APPLICATIONS INVOLVING IMPLANTATION IN THE HUMAN BODY OR
CONTACT WITH INTERNAL BODY FLUIDS OR TISSUES UNLESS THE MATERIAL HAS BEEN PROVIDED FROM DUPONT UNDER A
WRITTEN CONTRACT THAT IS CONSISTENT WITH DUPONT POLICY REGARDING MEDICAL APPLICATIONS AND EXPRESSLY
ACKNOWLEDGES THE CONTEMPLATED USE.
For further information, please contact your DuPont representative. You may also request a copy of DuPont POLICY Regarding Medical
Applications... H-50103-3 and DuPont CAUTION Regarding Medical Applications... H-50102-3.
Contact DuPont for Material Safety Data Sheet, general guides and/or additional information about ventilation, handling, purging, drying, etc.
Test temperatures are 23°C unless otherwise stated.
The DuPont Oval Logo, DuPont™, The miracles of science™ and ® are trademarks or registered trademarks of DuPont Company.
Copyright© 2011 E.I. du Pont de Nemours and Company. All Rights Reserved.
The information provided in this data sheet corresponds to our knowledge on the subject at the date of its publication.
This information may be subject to revision as new knowledge and experience becomes available.
The data provided fall within the normal range of product properties and relate only to the specific material designated; these data may not be
valid for such material used in combination with any other materials, additives or pigments or in any process, unless expressly indicated otherwise.
The data provided should not be used to establish specification limits or used alone as the basis of design; they are not intended to substitute
for any testing you may need to conduct to determine for yourself the suitability of a specific material for your particular purposes.
Since DuPont cannot anticipate all variations in actual end-use conditions DuPont makes no warranties and assumes no liability in connection
with any use of this information.
Nothing in this publication is to be considered as a license to operate under or a recommendation to infringe any patent rights.
DuPont advises you to seek independent counsel for a freedom to practice opinion on the intended application or end-use of our products.
CAUTION: DO NOT USE DUPONT MATERIALS IN MEDICAL APPLICATIONS INVOLVING IMPLANTATION IN THE HUMAN BODY OR
CONTACT WITH INTERNAL BODY FLUIDS OR TISSUES UNLESS THE MATERIAL HAS BEEN PROVIDED FROM DUPONT UNDER A
WRITTEN CONTRACT THAT IS CONSISTENT WITH DUPONT POLICY REGARDING MEDICAL APPLICATIONS AND EXPRESSLY
ACKNOWLEDGES THE CONTEMPLATED USE.
For further information, please contact your DuPont representative. You may also request a copy of DuPont POLICY Regarding Medical
Applications... H-50103-3 and DuPont CAUTION Regarding Medical Applications... H-50102-3.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012
CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012