CAMPUS® datasheet | Durethan® BM 240 H3.0


This datasheet of Durethan® BM 240 H3.0 from LANXESS Deutschland GmbH is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Durethan® BM 240 H3.0 | PA6-MD40 | LANXESS Deutschland GmbH
Product Texts
PA 6, 40 % mineral, injection moulding, heat-ageing stabilized, low tendency to warp, isotopic properties
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.8 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.8 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 5800 / 2200 MPa ISO 527-1/-2
Stress at break 85 / 55 MPa ISO 527-1/-2
Strain at break 6 / 40 % ISO 527-1/-2
Charpy impact strength (+23°C) 140 / N kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 80 / 80 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 10 / 12 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 10 / 10 kJ/m² ISO 179/1eA
Puncture - maximum force (+23°C) 3030 / - N ISO 6603-2
Puncture - maximum force (-30°C) 728 / - N ISO 6603-2
Puncture energy (+23°C) 20 / 65 J ISO 6603-2
Puncture energy (-30°C) 3 / 3 J ISO 6603-2
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 222 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 85 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 185 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 60 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 70 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Oxygen index 27 / * % ISO 4589-1/-2
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 4.5 / - - IEC 60250
Relative permittivity (1MHz) 4 / - - IEC 60250
Dissipation factor (100Hz) 250 / - E-4 IEC 60250
Dissipation factor (1MHz) 240 / - E-4 IEC 60250
Volume resistivity 1E13 / - Ohm*m IEC 60093
Electric strength 35 / - kV/mm IEC 60243-1
Comparative tracking index 550 / - - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 6 / * % Sim. to ISO 62
Humidity absorption 1.9 / * % Sim. to ISO 62
Density 1450 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
Viscosity number 142 / * cm³/g ISO 307, 1157, 1628
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1240 kg/m³ -
Thermal conductivity of melt 0.247 W/(m K) -
Spec. heat capacity melt 1990 J/(kg K) -
Eff. thermal diffusivity 1E-7 m²/s -
Ejection temperature 140 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 290 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Diagrams
Viscosity-shear rate , Durethan® BM 240 H3.0, PA6-MD40, LANXESS
Shearstress-shear rate , Durethan® BM 240 H3.0, PA6-MD40, LANXESS
Dynamic Shear modulus-temperature , Durethan® BM 240 H3.0, PA6-MD40, LANXESS
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding

PREPROCESSING
Max. Water content: 0.1 %
Drying temperature: 80 °C

 

Drying time:
Dry air dryer     2-20 h (will depend on the initial moisture content)

 

PROCESSING
Melt temperature:    270 - 290 °C
Mold temperature:     80 - 120 °C

Disclaimer
This information and our  technical advice - whether verbal, in  writing
or by way of trials - are  given in good faith but without warranty, and
this  also  applies  where  proprietary  rights  of  third  parties  are
involved.  Our advice does not release you from  the obligation to check
its validity and to test our  products  as to their  suitability for the
intended processes and uses.  The  application, use  and  processing  of
our products and the products manufactured  by  you  on the basis of our
technical  advice  are  beyond our control and, therefore, entirely your
own  responsibility.  Our  products  are  sold  in  accordance  with our
General  Conditions of Sale and Delivery.
The values  stored in the databank should only be used as guidelines for
component   design.  In  giving  these  values  neither  guarantee,  nor
assurance of particular material properties can be given.

techcenter.lanxess.com

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991