  Durethan® DP BC 310 EF | PA6 | LANXESS Deutschland GmbH
Product Texts
PA 6, injection molding and extrusion grade, non-reinforced, elastomer modified, high impact strength, good flowability (EasyFlow)
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.8 / * % ISO 294-4, 2577
Molding shrinkage (normal) 1.1 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 2300 / - MPa ISO 527-1/-2
Yield stress 50 / - MPa ISO 527-1/-2
Yield strain 3.8 / - % ISO 527-1/-2
Charpy impact strength (+23°C) 195 / - kJ/m² ISO 179/1eU
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 220 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 63 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 158 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion (parallel) 80 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 140 / * E-6/K ISO 11359-1/-2
Other propertiesdry / condUnitTest Standard
Water absorption 7.4 / * % Sim. to ISO 62
Density 1120 / - kg/m³ ISO 1183
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets
Regional Availability
Other text information
Injection molding

PREPROCESSING
Max. Water content: 0.1 %
Drying temperature: 80 °C

 

Drying time:
Dry air dryer     2-20 h (will depend on the initial moisture content)

 

PROCESSING
Melt temperature:    260 - 280 °C
Mold temperature:     80 - 90 °C

Disclaimer
This information and our  technical advice - whether verbal, in  writing
or by way of trials - are  given in good faith but without warranty, and
this  also  applies  where  proprietary  rights  of  third  parties  are
involved.  Our advice does not release you from  the obligation to check
its validity and to test our  products  as to their  suitability for the
intended processes and uses.  The  application, use  and  processing  of
our products and the products manufactured  by  you  on the basis of our
technical  advice  are  beyond our control and, therefore, entirely your
own  responsibility.  Our  products  are  sold  in  accordance  with our
General  Conditions of Sale and Delivery.
The values  stored in the databank should only be used as guidelines for
component   design.  In  giving  these  values  neither  guarantee,  nor
assurance of particular material properties can be given.

techcenter.lanxess.com

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991