Designation: Thermoplastics ISO 2897-PS-I,M,088-06-04-18
UL94 V-0, polybromobiphenylether (PBBE) free, flame retarded, high impact polystyrene.
This grade combines medium flow, heat resistance and good light stability for injection moulding of technical parts.
Applications:
Printers and copiers, ventilators, TV back covers, business machines,
monitor cabinets.
| Rheological properties | Value | Unit | Test Standard |
| Melt volume-flow rate (MVR) | 3.7 | cm³/10min | ISO 1133 |
| Temperature | 200 | °C | ISO 1133 |
| Load | 5 | kg | ISO 1133 |
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 1950 | MPa | ISO 527-1/-2 |
| Yield stress | 21 | MPa | ISO 527-1/-2 |
| Yield strain | 1.3 | % | ISO 527-1/-2 |
| Nominal strain at break | 45 | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | 70 | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 7 | kJ/m² | ISO 179/1eA |
| Thermal properties | Value | Unit | Test Standard |
| Glass transition temperature (10°C/min) | 95 | °C | ISO 11357-1/-2 |
| Temp. of deflection under load (1.80 MPa) | 74 | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 89 | °C | ISO 306 |
| Coeff. of linear therm. expansion (parallel) | 90 | E-6/K | ISO 11359-1/-2 |
| Burning Behav. at 1.5 mm nom. thickn. | V-0 | class | IEC 60695-11-10 |
| Thickness tested | 1.5 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Burning Behav. at thickness h | V-0 | class | IEC 60695-11-10 |
| Thickness tested | 6.0 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Burning Behav. 5V at thickness h | 5VA | class | IEC 60695-11-20 |
| Thickness tested | 6.0 | mm | IEC 60695-11-20 |
| UL recognition | UL | - | - |
| Electrical properties | Value | Unit | Test Standard |
| Relative permittivity (100Hz) | 2.5 | - | IEC 60250 |
| Relative permittivity (1MHz) | 2.5 | - | IEC 60250 |
| Dissipation factor (100Hz) | 4 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | 4 | E-4 | IEC 60250 |
| Volume resistivity | >1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | >1E15 | Ohm | IEC 60093 |
| Electric strength | 26 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 400 | - | IEC 60112 |
| Other properties | Value | Unit | Test Standard |
| Water absorption | 0.06 | % | Sim. to ISO 62 |
| Humidity absorption | 0.04 | % | Sim. to ISO 62 |
| Density | 1150 | kg/m³ | ISO 1183 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Density of melt | 1080 | kg/m³ | - |
| Spec. heat capacity melt | 1850 | J/(kg K) | - |
| Test specimen production | Value | Unit | Test Standard |
| Processing conditions acc. ISO | 2900 | - | ISO ....-2 |
| Injection Molding, melt temperature | 220 | °C | ISO 294 |
| Injection Molding, mold temperature | 45 | °C | ISO 10724 |
| Injection Molding, injection velocity | 200 | mm/s | ISO 294 |
| Injection Molding, pressure at hold | 70 | MPa | ISO 294 |
PREPROCESSING
Predrying recommended at 70 °C for 2 hours
PROCESSING
Typical processing temperature range:
Melt temperature 190 - 230 °C
Mold temperature 20 - 60 °C
Predrying recommended at 70 °C for 2 hours orvented barrel
PROCESSING
Melt temperature 190 - 230°C
PREPROCESSING
Predrying recommended at 70 °C for 2 hours orvented barrel
PROCESSING
Melt temperature 190 -230 °C
Predrying recommended at 70 °C for 2 hours orvented barrel
PROCESSING
Melt temperature 190 -230 °C
Dear CAMPUS User, The data, information and suggestions are provided for guidance purpose only. The Company accepts no responsibility for the results obtained therefrom, as neither for their utilisation in infringement of possible patents rights. All indicated data refer to natural grades. On the subject of the experimental products, the Company reserves the right to change without prewarning the characteristics, to optimise the performances. If you have any questions regarding CAMPUS, please send an e-mail to:Pe Campus For further information regarding Polimeri Europa: Polimeri Europa Homepage
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991