Elastollan® 1174 D | TPU | BASF Polyurethanes GmbH
Product Texts
DESCRIPTION
Elastollan 1174 D is a polyether based TPU
SPECIAL PROPERTIES
excellent resistance to hydrolysis and good flexibility at
low temperature, resistance to microbiological attack,
good wear performance, high tensile strength, good damping behavior
TYPICAL APPLICATIONS
ski binding elements, ski surface films
OTHER HINTS
predrying: 2-3h at 90-120°C
(air circulating oven or dehumidified air dryer),
max. content of humidity before processing: 0,02%
annealing: 20 h at 100°C in order to get optimum properties
For detailed information on medical and food applications
refer to this information brochure
CHEMICAL RESISTANCE
For detailed information on the chemical resistance of our
materials refer to this list of chemical resistance
Elastollan 1174 D is a polyether based TPU
SPECIAL PROPERTIES
excellent resistance to hydrolysis and good flexibility at
low temperature, resistance to microbiological attack,
good wear performance, high tensile strength, good damping behavior
TYPICAL APPLICATIONS
ski binding elements, ski surface films
OTHER HINTS
predrying: 2-3h at 90-120°C
(air circulating oven or dehumidified air dryer),
max. content of humidity before processing: 0,02%
annealing: 20 h at 100°C in order to get optimum properties
For detailed information on medical and food applications
refer to this information brochure
CHEMICAL RESISTANCE
For detailed information on the chemical resistance of our
materials refer to this list of chemical resistance
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 560 | MPa | ISO 527-1/-2 |
| Stress at 50% strain | 26 | MPa | ISO 527-1/-2 |
| Stress at 100% elongation | 30 | MPa | ISO 527-1/-2 |
| Stress at 300% elongation | 45 | MPa | ISO 527-1/-2 |
| Stress at break TPE | 50 | MPa | ISO 527-1/-2 |
| Strain at break | >50 | % | ISO 527-1/-2 |
| Strain at break TPE | >300 | % | ISO 527-1/-2 |
| Charpy notched impact strength (+23°C) | N | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | 5 | kJ/m² | ISO 179/1eA |
| Tensile notched impact strength (+23°C) | 360 | kJ/m² | ISO 8256/1 |
| Compression Set under constant strain (23°C) | 50 | % | ISO 815 |
| Compression Set under constant strain (70°C) | 55 | % | ISO 815 |
| Tear strength | 220 | kN/m | ISO 34-1 |
| Abrasion resistance | 25 | mm³ | ISO 4649 |
| Shore D hardness (15s) | 72 | - | ISO 868 |
| Thermal properties | Value | Unit | Test Standard |
| Glass transition temperature (10°C/min) | 6 | °C | ISO 11357-1/-2 |
| Temp. of deflection under load (1.80 MPa) | 50 | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 81 | °C | ISO 75-1/-2 |
| Coeff. of linear therm. expansion (normal) | 100 | E-6/K | ISO 11359-1/-2 |
| Electrical properties | Value | Unit | Test Standard |
| Dissipation factor (100Hz) | 330 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | 420 | E-4 | IEC 60250 |
| Volume resistivity | 1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | >1E15 | Ohm | IEC 60093 |
| Electric strength | 37 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 600 | - | IEC 60112 |
| Other properties | Value | Unit | Test Standard |
| Density | 1200 | kg/m³ | ISO 1183 |
| Test specimen production | Value | Unit | Test Standard |
| Injection Molding, melt temperature | 240 | °C | ISO 294 |
| Injection Molding, mold temperature | 60 | °C | ISO 10724 |
Diagrams
Characteristics
Processing
Injection Molding, Profile Extrusion
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
Barrel temperature : 220 - 235 °C
Melt temperature : 235 °C
Mold temperature: 25 - 40 °C
Melt temperature : 235 °C
Mold temperature: 25 - 40 °C
Disclaimer
The data contained in this publication are based on
our current knowledge and experience. In view of
the many factors that may affect processing and
application of our product, these data do not relieve
processors from carrying out their own investigations
and tests. Any descriptions, drawings, photographs,
data, proportions, weights etc. given herein may
change without prior information and do not constitute
the agreed contractual quality of the product. It is
the responsibility of the recipient of our products
to ensure that any proprietary rights and existing
laws and legislation are observed. NO WARRANTIES
OF ANY KIND, EITHER EXPRESS OR IMPLIED,
INCLUDING WARRANTIES OFMERCHANTABILITY OR
FITNESS FOR A PARTICULAR PURPOSE, ARE MADE
REGARDING PRODUCTS DESCRIBED OR DESIGNS,
DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY
BE USED WITHOUT INFRINGING THEINTELLECTUAL
PROPERTY RIGHTS OF OTHERS.
In order to check the availability of products please
contact us or our sales agency.
For more information about our products contact your
local BASF representative or
BASF Polyurethanes GmbH
European Business Management
Thermoplastische Polyurethane
Elastogranstraße 60
D-49448 Lemförde
Deutschland
Telefon ++49 5443 122500
Telefax ++49 5443 122555
e-mail: pu-elastomere@basf.com
www.pu.basf.de CAMPUS® is a registered trademark of CWFG (Chemie Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991