View list of
  • All BASF PU grades
  • All TPU grades
  • All grades beginning with E

CAMPUS® datasheet | Elastollan® 1175 A W


This datasheet of Elastollan® 1175 A W from BASF Polyurethanes GmbH is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Elastollan® 1175 A W | TPU | BASF Polyurethanes GmbH
Product Texts
DESCRIPTION
Elastollan 1175 AW is a polyether based TPU with plasticiser

SPECIAL PROPERTIES
excellent resistance to hydrolysis and good flexibility at low temperature,
resistance to microbiological attack, good wear performance,
high tensile strength, good damping behavior

TYPICAL APPLICATIONS
cable sheathing, plugs and terminations, hoses, damping elements

OTHER HINTS
predrying: 2-3h at 70-85°C (dehumidified air dryer),
max. content of humidity before processing: 0,02%
annealing: 20 h at 100°C in order to get optimum properties

CHEMICAL RESISTANCE
For detailed information on the chemical resistance of our
materials refer to this list of chemical resistance
Mechanical propertiesValueUnitTest Standard
Stress at 50% strain 3 MPa ISO 527-1/-2
Stress at 100% elongation 4 MPa ISO 527-1/-2
Stress at 300% elongation 8 MPa ISO 527-1/-2
Stress at break TPE 40 MPa ISO 527-1/-2
Strain at break >50 % ISO 527-1/-2
Strain at break TPE >300 % ISO 527-1/-2
Compression Set under constant strain (23°C) 20 % ISO 815
Compression Set under constant strain (70°C) 40 % ISO 815
Tear strength 40 kN/m ISO 34-1
Abrasion resistance 45 mm³ ISO 4649
Shore A hardness (3s) 75 - ISO 868
Thermal propertiesValueUnitTest Standard
Glass transition temperature (10°C/min) -46 °C ISO 11357-1/-2
Burning Behav. at 1.5 mm nom. thickn. V-2 class IEC 60695-11-10
Burning Behav. at thickness h V-0 class IEC 60695-11-10
Oxygen index 25 % ISO 4589-1/-2
Electrical propertiesValueUnitTest Standard
Dissipation factor (1MHz) 1100 E-4 IEC 60250
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Density 1140 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 200 °C ISO 294
Injection Molding, mold temperature 60 °C ISO 10724
Diagrams
Viscosity-shear rate , Elastollan® 1175 A W, TPU, BASF PU
Shearstress-shear rate , Elastollan® 1175 A W, TPU, BASF PU
Dynamic Shear modulus-temperature , Elastollan® 1175 A W, TPU, BASF PU
Stress-Strain (TPE) , Elastollan® 1175 A W, TPU, BASF PU
Characteristics
Processing
Injection Molding, Profile Extrusion
Delivery form
Pellets
Additives
Plasticizer
Regional Availability
Other text information
Injection molding
Barrel temperature : 195 - 205 °C
Melt temperature : 205 °C
Mold temperature: 25 - 40 °C
Profile extrusion
Barrel temperature : 160 - 175 °C
Disclaimer
The data contained in this publication are based on
our current knowledge and experience. In view of
the many factors that may affect processing and
application of our product, these data do not relieve
processors from carrying out their own investigations
and tests.  Any descriptions, drawings, photographs,
data, proportions, weights etc. given herein may
change without prior information and do not constitute
the agreed contractual quality of the product. It is
the responsibility of the recipient  of our products
to ensure that any proprietary rights and existing
laws and legislation are observed. NO WARRANTIES
OF ANY KIND, EITHER EXPRESS OR IMPLIED,
INCLUDING WARRANTIES OFMERCHANTABILITY OR
FITNESS FOR A PARTICULAR PURPOSE, ARE MADE
REGARDING PRODUCTS DESCRIBED OR DESIGNS,
DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY
BE USED WITHOUT INFRINGING THEINTELLECTUAL
PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please
contact us or our sales agency.


For more information about our products contact your
local BASF representative or

    BASF Polyurethanes GmbH
    European Business Management
    Thermoplastische Polyurethane
    Elastogranstraße 60
    D-49448 Lemförde
    Deutschland
    Telefon ++49 5443 122500
    Telefax ++49 5443 122555
    e-mail: pu-elastomere@basf.com
    www.pu.basf.de 
CAMPUS® is a registered trademark of CWFG (Chemie Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt) 

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991