offers extended functionality!CAMPUS® datasheet | FORTRON 0320
This datasheet of FORTRON 0320 from Ticona is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
FORTRON 0320 | PPS | Ticona
Product Texts
0320 exhibits a high melt strength for extrusion processes. The
material demonstrates excellent heat and chemical resistance. The
intended use of this product is for extruding monofilament/fibers, rod
and slab. Available standard in powder (0320B0), pellet (0320P0) and
crystallized pellet (0320C0) form.
material demonstrates excellent heat and chemical resistance. The
intended use of this product is for extruding monofilament/fibers, rod
and slab. Available standard in powder (0320B0), pellet (0320P0) and
crystallized pellet (0320C0) form.
| Thermal properties | Value | Unit | Test Standard |
| Melting temperature (10°C/min) | 280 | °C | ISO 11357-1/-3 |
| Glass transition temperature (10°C/min) | 90 | °C | ISO 11357-1/-2 |
| Temp. of deflection under load (1.80 MPa) | 115 | °C | ISO 75-1/-2 |
| Temp. of deflection under load (8.00 MPa) | 95 | °C | ISO 75-1/-2 |
| Coeff. of linear therm. expansion (parallel) | 52 | E-6/K | ISO 11359-1/-2 |
| Coeff. of linear therm. expansion (normal) | 53 | E-6/K | ISO 11359-1/-2 |
| Burning Behav. at thickness h | V-0 | class | IEC 60695-11-10 |
| Thickness tested | 3.0 | mm | IEC 60695-11-10 |
| Electrical properties | Value | Unit | Test Standard |
| Relative permittivity (1MHz) | 4.6 | - | IEC 60250 |
| Dissipation factor (1MHz) | 11 | E-4 | IEC 60250 |
| Volume resistivity | 1E9 | Ohm*m | IEC 60093 |
| Electric strength | 18 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 125 | - | IEC 60112 |
| Other properties | Value | Unit | Test Standard |
| Water absorption | 0.02 | % | Sim. to ISO 62 |
| Density | 1350 | kg/m³ | ISO 1183 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Spec. heat capacity melt | 1830 | J/(kg K) | - |
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Sheet Extrusion, Other Extrusion
Delivery form
Pellets, Powder
Regional Availability
Other text information
Injection molding
PREPROCESSING
In spite of the minimum moisture absorption a drying of FORTRON is
necessary. Predrying in a dehumidified air dryer at 120 degC/3-4 hours
is recommended.
PROCESSING
On injection molding machines with 15-25 D long three-section screws,
are usual in the trade, the unreinforced FORTRON is processable. A
shut-off nozzle is recommended.
Melt temperature 310-320 degC
Mold wall temperature at least 140 degC
A m edium injection rate is normally preferred. All mold cavities must
be effectively vented.
POSTPROCESSING
In spite of the minimum moisture absorption a drying of FORTRON is
necessary. Predrying in a dehumidified air dryer at 120 degC/3-4 hours
is recommended.
PROCESSING
On injection molding machines with 15-25 D long three-section screws,
are usual in the trade, the unreinforced FORTRON is processable. A
shut-off nozzle is recommended.
Melt temperature 310-320 degC
Mold wall temperature at least 140 degC
A m edium injection rate is normally preferred. All mold cavities must
be effectively vented.
POSTPROCESSING
Disclaimer
NOTICE TO USERS: Values shown are based on testing of laboratory test specimens and represent data that fall within the standard range of properties for natural material. These values alone do not represent a sufficient basis for any part design and are not intended for use in establishing maximum, minimum, or ranges of values for specification purposes. Colorants or other additives may cause significant variations in data values. Properties of molded parts can be influenced by a wide variety of factors including, but not limited to, material selection, additives, part design, processing conditions and environmental exposure. Any determination of the suitability of a particular material and part design for any use contemplated by the users and the manner of such use is the sole responsibility of the users, who must assure themselves that the material as subsequently processed meets the needs of their particular product or use. To the best of our knowledge, the information contained in this publication is accurate; however, we do not assume any liability whatsoever for the accuracy and completeness of such information. The information contained in this publication should not be construed as a promise or guarantee of specific properties of our products. It is the sole responsibility of the users to investigate whether any existing patents are infringed by the use of the materials mentioned in this publication. Moreover, there is a need to reduce human exposure to many materials to the lowest practical limits in view of possible adverse effects. To the extent that any hazards may have been mentioned in this publication, we neither suggest nor guarantee that such hazards are the only ones which exist. We recommend that persons intending to rely on any recommendation or to use any equipment, processing technique, or material mentioned in this publication should satisfy themselves that they can meet all applicable safety and health standards. We strongly recommend that users seek and adhere to the manufacturer's current instructions for handling each material they use, and to entrust the handling of such material to adequately trained personnel only. Please call the telephone numbers listed for additional technical information. Call Customer Services for the appropriate Materials Safety Data Sheets (MSDS) before attempting to process our products. The products mentioned herein are not intended for use in medical or dental implants.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.