View list of

CAMPUS® datasheet | Grilamid L 20 G


This datasheet of Grilamid L 20 G from EMS-GRIVORY | a unit of EMS-CHEMIE AG is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Grilamid L 20 G | PA12 | EMS-GRIVORY | a unit of EMS-CHEMIE AG
Product Texts
Product designation according to ISO 1874: PA12, MHR, 18-010

 

Markets

  Automotive
  Powertrain and Chassis
  Electricals & Electronics
  Connectors
  Industry & Consumer goods
  Housewares, Mechanical Engineering, Medical devices, Sports & Leisure, Tools & Accessories

Approvals

  Water contact
  DVGW W270
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.8 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.8 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 1600 / 1100 MPa ISO 527-1/-2
Yield stress 50 / 40 MPa ISO 527-1/-2
Yield strain 5 / 12 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) N / N kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) N / N kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 5 / 7 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 6 / 6 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 178 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 45 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 115 / * °C ISO 75-1/-2
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Volume resistivity - / 1E11 Ohm*m IEC 60093
Surface resistivity * / 1E12 Ohm IEC 60093
Electric strength - / 32 kV/mm IEC 60243-1
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 1.5 / * % Sim. to ISO 62
Humidity absorption 0.7 / * % Sim. to ISO 62
Density 1010 / - kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 860 kg/m³ -
Thermal conductivity of melt 0.22 W/(m K) -
Spec. heat capacity melt 2900 J/(kg K) -
Eff. thermal diffusivity 8.82E-8 m²/s -
Ejection temperature 140 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 250 °C ISO 294
Injection Molding, mold temperature 40 °C ISO 10724
Injection Molding, injection velocity 250 mm/s ISO 294
Injection Molding, pressure at hold 75 MPa ISO 294
Diagrams
Viscosity-shear rate , Grilamid L 20 G, PA12, EMS-GRIVORY
Shearstress-shear rate , Grilamid L 20 G, PA12, EMS-GRIVORY
Dynamic Shear modulus-temperature , Grilamid L 20 G, PA12, EMS-GRIVORY
Stress-strain , Grilamid L 20 G, PA12, EMS-GRIVORY
Secant modulus-strain , Grilamid L 20 G, PA12, EMS-GRIVORY
Stress-strain (isochronous) 23°C, Grilamid L 20 G, PA12, EMS-GRIVORY
Creep modulus-time 23°C, Grilamid L 20 G, PA12, EMS-GRIVORY
Specific volume-temperature (pvT) , Grilamid L 20 G, PA12, EMS-GRIVORY
Tensile modulus-temperature , Grilamid L 20 G, PA12, EMS-GRIVORY
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Max. water content : <= 0.1 %
PROCESSING
Melt temperature : 250 °C
Mould wall temperature : 40 °C
Holding pressure : 300-800 bar
Screw : 50-100 rpm
Back pressure : 1-15 bar
Injection speed : 2
(1=slow, 3=medium, 5=fast)

Please consider the information about the application of the materials.
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Citric Acid solution (10% by mass) (23°C)
Lactic Acid (10% by mass) (23°C)
Hydrochloric Acid (36% by mass) (23°C)
Nitric Acid (40% by mass) (23°C)
Sulfuric Acid (38% by mass) (23°C)
Sulfuric Acid (5% by mass) (23°C)
Chromic Acid solution (40% by mass) (23°C)
Bases
Sodium Hydroxide solution (35% by mass) (23°C)
Sodium Hydroxide solution (1% by mass) (23°C)
Ammonium Hydroxide solution (10% by mass) (23°C)
Alcohols
Isopropyl alcohol (23°C)
Methanol (23°C)
Ethanol (23°C)
Hydrocarbons
n-Hexane (23°C)
Toluene (23°C)
iso-Octane (23°C)
Ketones
Acetone (23°C)
Ethers
Diethyl ether (23°C)
Mineral oils
SAE 10W40 multigrade motor oil (23°C)
SAE 10W40 multigrade motor oil (130°C)
SAE 80/90 hypoid-gear oil (130°C)
Insulating Oil (23°C)
Standard Fuels
ISO 1817 Liquid 1 (60°C)
ISO 1817 Liquid 2 (60°C)
ISO 1817 Liquid 3 (60°C)
ISO 1817 Liquid 4 (60°C)
Standard fuel without alcohol (pref. ISO 1817 Liquid C) (23°C)
Standard fuel with alcohol (pref. ISO 1817 Liquid 4) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (90°C)
Diesel fuel (pref. ISO 1817 Liquid F) (>90°C)
Salt solutions
Sodium Chloride solution (10% by mass) (23°C)
Sodium Hypochlorite solution (10% by mass) (23°C)
Sodium Carbonate solution (20% by mass) (23°C)
Sodium Carbonate solution (2% by mass) (23°C)
Zinc Chloride solution (50% by mass) (23°C)
Other
Ethyl Acetate (23°C)
Hydrogen peroxide (23°C)
DOT No. 4 Brake fluid (130°C)
Ethylene Glycol (50% by mass) in water (108°C)
1% nonylphenoxy-polyethyleneoxy ethanol in water (23°C)
50% Oleic acid + 50% Olive Oil (23°C)
Water (23°C)
Deionized water (90°C)
Phenol solution (5% by mass) (23°C)
Disclaimer
EMS-CHEMIE AG
Business Unit EMS-GRIVORY

Homepage : EMS-GRIVORY
eMail    : welcome@emsgrivory.com


In the line with the aims of CAMPUS, the values are intended to serve as
an aid in preselecting materials and  for an overview of the EMS-GRIVORY
product  range.  They  correspond  to our  current  knowledge,  a  legal
guarantee concerning the application and the manufacture can however not
be assumed.  This data does not  cancel the processor's  own testing and
inspection obligations.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991