CAMPUS® datasheet | Grilamid LV-3H


This datasheet of Grilamid LV-3H from EMS-GRIVORY | a unit of EMS-CHEMIE AG is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Grilamid LV-3H | PA12-GF30 | EMS-GRIVORY | a unit of EMS-CHEMIE AG
Product Texts
Product designation according to ISO 1874: PA12, MHR, 18-060, GF30

 

Product Attributes

  Hydrolysis resistant, Improved impact resistance, Improved heat resistance,
Improved UV resistance (outdoor use)

Markets

  Automotive
  Air intake sytems, Compressed air systems, Hydraulic systems,
Automotive electr. and electronics, lighting, Cooling and climate control, Fuel systems, Powertrain and Chassis
  Electricals & Electronics
  Electrical appliances, Connectors, Mobile phones and other portable devices
  Industry & Consumer goods
  Heating systems, Housewares, Hydraulics & Pneumatics, Mechanical Engineering, Medical devices,
Power transmission, Sanitary, water and gas supply, Sports & Leisure, Tools & Accessories

Approvals

  Water contact
  DVGW W270
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.1 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.8 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 6500 / 6000 MPa ISO 527-1/-2
Stress at break 120 / 105 MPa ISO 527-1/-2
Strain at break 6 / 8 % ISO 527-1/-2
Charpy impact strength (+23°C) 90 / 80 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 90 / 80 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 19 / 20 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 15 / 15 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 178 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 160 / * °C ISO 75-1/-2
Temp. of deflection under load (8.00 MPa) 90 / * °C ISO 75-1/-2
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Volume resistivity - / 1E11 Ohm*m IEC 60093
Surface resistivity * / 1E12 Ohm IEC 60093
Electric strength - / 35 kV/mm IEC 60243-1
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 1.1 / * % Sim. to ISO 62
Humidity absorption 0.6 / * % Sim. to ISO 62
Density 1220 / - kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1050 kg/m³ -
Thermal conductivity of melt 0.26 W/(m K) -
Spec. heat capacity melt 2200 J/(kg K) -
Eff. thermal diffusivity 1.13E-7 m²/s -
Ejection temperature 155 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Injection Molding, injection velocity 300 mm/s ISO 294
Injection Molding, pressure at hold 75 MPa ISO 294
Diagrams
Viscosity-shear rate , Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Shearstress-shear rate , Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Dynamic Shear modulus-temperature , Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Stress-strain , Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Secant modulus-strain , Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Stress-strain (isochronous) 23°C, Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Creep modulus-time 23°C, Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Tensile modulus-temperature , Grilamid LV-3H, PA12-GF30, EMS-GRIVORY
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Max. water content : <= 0.1 %
PROCESSING
Melt temperature : 260 °C
Mould wall temperature : 80 °C
Holding pressure : 300-800 bar
Screw : 50-100 rpm
Back pressure : 1-15 bar
Injection speed : 4
(1=slow, 3=medium, 5=fast)

Please consider the information about the application of the materials.
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Citric Acid solution (10% by mass) (23°C)
Lactic Acid (10% by mass) (23°C)
Hydrochloric Acid (36% by mass) (23°C)
Nitric Acid (40% by mass) (23°C)
Sulfuric Acid (38% by mass) (23°C)
Sulfuric Acid (5% by mass) (23°C)
Chromic Acid solution (40% by mass) (23°C)
Bases
Sodium Hydroxide solution (35% by mass) (23°C)
Sodium Hydroxide solution (1% by mass) (23°C)
Ammonium Hydroxide solution (10% by mass) (23°C)
Alcohols
Isopropyl alcohol (23°C)
Methanol (23°C)
Ethanol (23°C)
Hydrocarbons
n-Hexane (23°C)
Toluene (23°C)
iso-Octane (23°C)
Ketones
Acetone (23°C)
Ethers
Diethyl ether (23°C)
Mineral oils
SAE 10W40 multigrade motor oil (23°C)
SAE 10W40 multigrade motor oil (130°C)
SAE 80/90 hypoid-gear oil (130°C)
Insulating Oil (23°C)
Standard Fuels
ISO 1817 Liquid 1 (60°C)
ISO 1817 Liquid 2 (60°C)
ISO 1817 Liquid 3 (60°C)
ISO 1817 Liquid 4 (60°C)
Standard fuel without alcohol (pref. ISO 1817 Liquid C) (23°C)
Standard fuel with alcohol (pref. ISO 1817 Liquid 4) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (90°C)
Diesel fuel (pref. ISO 1817 Liquid F) (>90°C)
Salt solutions
Sodium Chloride solution (10% by mass) (23°C)
Sodium Hypochlorite solution (10% by mass) (23°C)
Sodium Carbonate solution (20% by mass) (23°C)
Sodium Carbonate solution (2% by mass) (23°C)
Zinc Chloride solution (50% by mass) (23°C)
Other
Ethyl Acetate (23°C)
Hydrogen peroxide (23°C)
DOT No. 4 Brake fluid (130°C)
Ethylene Glycol (50% by mass) in water (108°C)
1% nonylphenoxy-polyethyleneoxy ethanol in water (23°C)
50% Oleic acid + 50% Olive Oil (23°C)
Water (23°C)
Deionized water (90°C)
Phenol solution (5% by mass) (23°C)
Disclaimer
EMS-CHEMIE AG
Business Unit EMS-GRIVORY

Homepage : EMS-GRIVORY
eMail    : welcome@emsgrivory.com


In the line with the aims of CAMPUS, the values are intended to serve as
an aid in preselecting materials and  for an overview of the EMS-GRIVORY
product  range.  They  correspond  to our  current  knowledge,  a  legal
guarantee concerning the application and the manufacture can however not
be assumed.  This data does not  cancel the processor's  own testing and
inspection obligations.