View list of

CAMPUS® datasheet | Grilamid LV-65H SST nat


This datasheet of Grilamid LV-65H SST nat from EMS-GRIVORY | a unit of EMS-CHEMIE AG is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Grilamid LV-65H SST nat | PA12-GF65 | EMS-GRIVORY | a unit of EMS-CHEMIE AG
Product Texts
Product designation according to ISO 1874: PA12, MHR, 18-190, GF65

 

Product Attributes

  Improved impact resistance, Improved heat resistance, Improved UV resistance (outdoor use)

Markets

  Automotive
  Compressed air systems, Hydraulic systems, Automotive electr. and electronics, lighting,
Powertrain and Chassis
  Electricals & Electronics
  Electrical appliances, Electrical equipment, Connectors, Mobile phones and other portable devices
  Industry & Consumer goods
  Housewares, Hydraulics & Pneumatics, Mechanical Engineering, Medical devices, Power transmission,
Sanitary, water and gas supply, Sports & Leisure, Tools & Accessories

Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.1 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.5 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 19000 / 18000 MPa ISO 527-1/-2
Stress at break 190 / 180 MPa ISO 527-1/-2
Strain at break 3 / 3.5 % ISO 527-1/-2
Charpy impact strength (+23°C) - / 75 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) - / 75 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) - / 13 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) - / 13 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 178 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 165 / * °C ISO 75-1/-2
Temp. of deflection under load (8.00 MPa) 150 / * °C ISO 75-1/-2
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Volume resistivity - / 1E11 Ohm*m IEC 60093
Surface resistivity * / 1E12 Ohm IEC 60093
Electric strength - / 35 kV/mm IEC 60243-1
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 0.7 / * % Sim. to ISO 62
Humidity absorption 0.3 / * % Sim. to ISO 62
Density 1700 / - kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1410 kg/m³ -
Thermal conductivity of melt 0.29 W/(m K) -
Spec. heat capacity melt 1900 J/(kg K) -
Eff. thermal diffusivity 1.08E-7 m²/s -
Ejection temperature 155 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 280 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Injection Molding, injection velocity 300 mm/s ISO 294
Injection Molding, pressure at hold 75 MPa ISO 294
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Disclaimer
EMS-CHEMIE AG
Business Unit EMS-GRIVORY

Homepage : EMS-GRIVORY
eMail    : welcome@emsgrivory.com


In the line with the aims of CAMPUS, the values are intended to serve as
an aid in preselecting materials and  for an overview of the EMS-GRIVORY
product  range.  They  correspond  to our  current  knowledge,  a  legal
guarantee concerning the application and the manufacture can however not
be assumed.  This data does not  cancel the processor's  own testing and
inspection obligations.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991