View list of

CAMPUS® datasheet | Grilamid TR 55


This datasheet of Grilamid TR 55 from EMS-GRIVORY | a unit of EMS-CHEMIE AG is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Grilamid TR 55 | PA12/MACMI | EMS-GRIVORY | a unit of EMS-CHEMIE AG
Product Texts
Product designation according to ISO 1874: PA 12/MACMI, GT, 11-020

 

Product Attributes

  Transparent

Markets

  Automotive
  Automotive electr. and electronics, lighting, Cooling and climate control, Fuel systems,
Powertrain and Chassis , Interior
  Electricals & Electronics
  Electrical appliances, Electrical equipment, Cables & Tubes, Energy distribution,
Mobile phones and other portable devices, Lighting
  Industry & Consumer goods
  Heating systems, Housewares, Hydraulics & Pneumatics, Mechanical Engineering, Medical devices,
Power transmission, Sanitary, water and gas supply, Sports & Leisure, Tools & Accessories
  Optics
  Lenses, Optical components
  Packaging
  Non oriented film, Cosmetics / Personal care, Medical packaging

Approvals

  Burning Behaviour
  UL V2
  Food Contact
  EU Requirements, FDA
  Medical
  USP VI, FDA
  Water contact
  NSF 61, KTW, WRAS, DVGW W270
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.6 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.7 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 2200 / 2200 MPa ISO 527-1/-2
Yield stress 75 / 75 MPa ISO 527-1/-2
Yield strain 7 / 9 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) N / N kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) N / N kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 7 / 8 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 7 / 7 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Glass transition temperature (10°C/min) 160 / * °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 130 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 145 / * °C ISO 75-1/-2
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Volume resistivity - / 1E11 Ohm*m IEC 60093
Surface resistivity * / 1E12 Ohm IEC 60093
Electric strength - / 31 kV/mm IEC 60243-1
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 3.5 / * % Sim. to ISO 62
Humidity absorption 1.5 / * % Sim. to ISO 62
Density 1060 / - kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1000 kg/m³ -
Thermal conductivity of melt 0.2 W/(m K) -
Spec. heat capacity melt 2100 J/(kg K) -
Eff. thermal diffusivity 9.52E-8 m²/s -
Ejection temperature 155 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 295 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Injection Molding, injection velocity 250 mm/s ISO 294
Injection Molding, pressure at hold 75 MPa ISO 294
Diagrams
Viscosity-shear rate , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Shearstress-shear rate , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Dynamic Shear modulus-temperature , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Stress-strain , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Secant modulus-strain , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Stress-strain (isochronous) 23°C, Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Creep modulus-time 23°C, Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Specific volume-temperature (pvT) , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Tensile modulus-temperature , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Stress-Strain (Film Grades) , Grilamid TR 55, PA12/MACMI, EMS-GRIVORY
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets
Special Characteristics
Transparent
Regional Availability
Other text information
Injection molding
PREPROCESSING
Max. water content : <= 0.08 %
PROCESSING
Melt temperature : 295 °C
Mould wall temperature : 80-120 °C
Holding pressure : 300-600 bar
Screw : 50-100 rpm
Back pressure : 1-15 bar
Injection speed : 3
(1=slow, 3=medium, 5=fast)

Please consider the information about the application of the materials.
Film extrusion
PREPROCESSING
Max. water content : <=0.08 %
PROCESSING
Melt temperature : 260-280 °C
Smooth or roughened feeding zone : 60-90 °C
Barrel temp. profile : 250-260 °C
Head temp. : 260-250 °C

Please consider the information about the application of the materials.
Other extrusion
-- PIPE EXTRUSION --
-- SHEATING --
PROCESSING
Melt temperature : 250-270 °C
Feeding bush : 60-90
Barrel temp. profile : 240-250 °C
Head temp. : 250-240 °C

Please consider the information about the application of the materials.
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Citric Acid solution (10% by mass) (23°C)
Lactic Acid (10% by mass) (23°C)
Hydrochloric Acid (36% by mass) (23°C)
Nitric Acid (40% by mass) (23°C)
Sulfuric Acid (38% by mass) (23°C)
Sulfuric Acid (5% by mass) (23°C)
Chromic Acid solution (40% by mass) (23°C)
Bases
Sodium Hydroxide solution (35% by mass) (23°C)
Sodium Hydroxide solution (1% by mass) (23°C)
Ammonium Hydroxide solution (10% by mass) (23°C)
Alcohols
Isopropyl alcohol (23°C)
Methanol (23°C)
Ethanol (23°C)
Hydrocarbons
n-Hexane (23°C)
Toluene (23°C)
iso-Octane (23°C)
Ketones
Acetone (23°C)
Ethers
Diethyl ether (23°C)
Mineral oils
SAE 10W40 multigrade motor oil (23°C)
SAE 10W40 multigrade motor oil (130°C)
SAE 80/90 hypoid-gear oil (130°C)
Insulating Oil (23°C)
Standard Fuels
ISO 1817 Liquid 1 (60°C)
ISO 1817 Liquid 2 (60°C)
ISO 1817 Liquid 3 (60°C)
ISO 1817 Liquid 4 (60°C)
Standard fuel without alcohol (pref. ISO 1817 Liquid C) (23°C)
Standard fuel with alcohol (pref. ISO 1817 Liquid 4) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (90°C)
Diesel fuel (pref. ISO 1817 Liquid F) (>90°C)
Salt solutions
Sodium Chloride solution (10% by mass) (23°C)
Sodium Hypochlorite solution (10% by mass) (23°C)
Sodium Carbonate solution (20% by mass) (23°C)
Sodium Carbonate solution (2% by mass) (23°C)
Zinc Chloride solution (50% by mass) (23°C)
Other
Ethyl Acetate (23°C)
Hydrogen peroxide (23°C)
DOT No. 4 Brake fluid (130°C)
Ethylene Glycol (50% by mass) in water (108°C)
1% nonylphenoxy-polyethyleneoxy ethanol in water (23°C)
50% Oleic acid + 50% Olive Oil (23°C)
Water (23°C)
Deionized water (90°C)
Phenol solution (5% by mass) (23°C)
Disclaimer
EMS-CHEMIE AG
Business Unit EMS-GRIVORY

Homepage : EMS-GRIVORY
eMail    : welcome@emsgrivory.com


In the line with the aims of CAMPUS, the values are intended to serve as
an aid in preselecting materials and  for an overview of the EMS-GRIVORY
product  range.  They  correspond  to our  current  knowledge,  a  legal
guarantee concerning the application and the manufacture can however not
be assumed.  This data does not  cancel the processor's  own testing and
inspection obligations.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991