  Grilon TS V0 | PA666 | EMS-GRIVORY | a unit of EMS-CHEMIE AG
Product Texts
Product designation according to ISO 1874: PA 66+PA 6, MFHR, 14-040 N

 

Product Attributes

  Flame retardant

Markets

  Automotive
  Automotive electr. and electronics, lighting
  Electricals & Electronics
  Electrical appliances, Electrical equipment, Cables & Tubes, Connectors, Energy distribution,
Lighting

Approvals

  Burning Behaviour
  UL V0
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.7 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.8 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 3600 / 1600 MPa ISO 527-1/-2
Yield stress 85 / 50 MPa ISO 527-1/-2
Yield strain 4 / 15 % ISO 527-1/-2
Nominal strain at break 10 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) 75 / 100 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 70 / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 4 / 15 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 3 / 3 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 260 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 70 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 210 / * °C ISO 75-1/-2
Burning Behav. at 1.5 mm nom. thickn. V-0 / * class IEC 60695-11-10
Thickness tested 1.5 / * mm IEC 60695-11-10
Burning Behav. at thickness h V-0 / * class IEC 60695-11-10
Thickness tested 0.4 / * mm IEC 60695-11-10
Oxygen index 35 / * % ISO 4589-1/-2
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 3 / 8 - IEC 60250
Relative permittivity (1MHz) 3 / 4 - IEC 60250
Dissipation factor (100Hz) 50 / 1500 E-4 IEC 60250
Dissipation factor (1MHz) 150 / 700 E-4 IEC 60250
Volume resistivity 1E11 / 1E9 Ohm*m IEC 60093
Surface resistivity * / 1E10 Ohm IEC 60093
Electric strength 28 / 26 kV/mm IEC 60243-1
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 8 / * % Sim. to ISO 62
Humidity absorption 2.5 / * % Sim. to ISO 62
Density 1160 / - kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 950 kg/m³ -
Thermal conductivity of melt 0.22 W/(m K) -
Spec. heat capacity melt 2500 J/(kg K) -
Eff. thermal diffusivity 9.26E-8 m²/s -
Ejection temperature 200 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 280 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Injection Molding, pressure at hold 75 MPa ISO 294
Diagrams
Viscosity-shear rate , Grilon TS V0, PA666, EMS-GRIVORY
Shearstress-shear rate , Grilon TS V0, PA666, EMS-GRIVORY
Dynamic Shear modulus-temperature , Grilon TS V0, PA666, EMS-GRIVORY
Dynamic Shear modulus-temperature , Grilon TS V0, PA666, EMS-GRIVORY
Stress-strain , Grilon TS V0, PA666, EMS-GRIVORY
Stress-strain , Grilon TS V0, PA666, EMS-GRIVORY
Secant modulus-strain , Grilon TS V0, PA666, EMS-GRIVORY
Secant modulus-strain , Grilon TS V0, PA666, EMS-GRIVORY
Stress-strain (isochronous) 23°C, Grilon TS V0, PA666, EMS-GRIVORY
Creep modulus-time 23°C, Grilon TS V0, PA666, EMS-GRIVORY
Stress-strain (isochronous) 80°C, Grilon TS V0, PA666, EMS-GRIVORY
Creep modulus-time 80°C, Grilon TS V0, PA666, EMS-GRIVORY
Specific volume-temperature (pvT) , Grilon TS V0, PA666, EMS-GRIVORY
Tensile modulus-temperature , Grilon TS V0, PA666, EMS-GRIVORY
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Max. water content : <= 0.1 %
PROCESSING
Melt temperature : 260-270 °C
Mould wall temperature : 80 °C
Holding pressure : 300-800 bar
Screw : 50-100 rpm
Back pressure : 1-15 bar
Injection speed : 3
(1=slow, 3=medium, 5=fast)

Please consider the information about the application of the materials.
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Citric Acid solution (10% by mass) (23°C)
Lactic Acid (10% by mass) (23°C)
Hydrochloric Acid (36% by mass) (23°C)
Nitric Acid (40% by mass) (23°C)
Sulfuric Acid (38% by mass) (23°C)
Sulfuric Acid (5% by mass) (23°C)
Chromic Acid solution (40% by mass) (23°C)
Bases
Sodium Hydroxide solution (35% by mass) (23°C)
Sodium Hydroxide solution (1% by mass) (23°C)
Ammonium Hydroxide solution (10% by mass) (23°C)
Alcohols
Isopropyl alcohol (23°C)
Methanol (23°C)
Ethanol (23°C)
Hydrocarbons
n-Hexane (23°C)
Toluene (23°C)
iso-Octane (23°C)
Ketones
Acetone (23°C)
Ethers
Diethyl ether (23°C)
Mineral oils
SAE 10W40 multigrade motor oil (23°C)
SAE 10W40 multigrade motor oil (130°C)
SAE 80/90 hypoid-gear oil (130°C)
Insulating Oil (23°C)
Standard Fuels
ISO 1817 Liquid 1 (60°C)
ISO 1817 Liquid 2 (60°C)
ISO 1817 Liquid 3 (60°C)
ISO 1817 Liquid 4 (60°C)
Standard fuel without alcohol (pref. ISO 1817 Liquid C) (23°C)
Standard fuel with alcohol (pref. ISO 1817 Liquid 4) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (90°C)
Diesel fuel (pref. ISO 1817 Liquid F) (>90°C)
Salt solutions
Sodium Chloride solution (10% by mass) (23°C)
Sodium Hypochlorite solution (10% by mass) (23°C)
Sodium Carbonate solution (20% by mass) (23°C)
Sodium Carbonate solution (2% by mass) (23°C)
Zinc Chloride solution (50% by mass) (23°C)
Other
Ethyl Acetate (23°C)
Hydrogen peroxide (23°C)
DOT No. 4 Brake fluid (130°C)
Ethylene Glycol (50% by mass) in water (108°C)
1% nonylphenoxy-polyethyleneoxy ethanol in water (23°C)
50% Oleic acid + 50% Olive Oil (23°C)
Water (23°C)
Deionized water (90°C)
Phenol solution (5% by mass) (23°C)
Disclaimer
EMS-CHEMIE AG
Business Unit EMS-GRIVORY

Homepage : EMS-GRIVORY
eMail    : welcome@emsgrivory.com


In the line with the aims of CAMPUS, the values are intended to serve as
an aid in preselecting materials and  for an overview of the EMS-GRIVORY
product  range.  They  correspond  to our  current  knowledge,  a  legal
guarantee concerning the application and the manufacture can however not
be assumed.  This data does not  cancel the processor's  own testing and
inspection obligations.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991