Product Texts
Product designation according to ISO 1874: PA 6I/6T, FT, 12-030

 

Partially aromatic Polyamide

Product Attributes

  High viscosity, Transparent, Barrier Properties

Markets

  Packaging
  Blow moulded containers, Injectionstretchblowmoulded containers, Tubes, Cosmetics / Personal care

Approvals

  Food Contact
  EU Requirements, FDA
Rheological propertiesdry / condUnitTest Standard
Melt volume-flow rate (MVR) 12 / * cm³/10min ISO 1133
Temperature 275 / * °C ISO 1133
Load 5 / * kg ISO 1133
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 3000 / 3000 MPa ISO 527-1/-2
Yield stress 100 / 100 MPa ISO 527-1/-2
Yield strain 5 / 5 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Charpy notched impact strength (+23°C) 8 / 8 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 8 / 2 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Glass transition temperature (10°C/min) 125 / * °C ISO 11357-1/-2
Other propertiesdry / condUnitTest Standard
Water absorption 7 / * % Sim. to ISO 62
Humidity absorption 2 / * % Sim. to ISO 62
Density 1180 / - kg/m³ ISO 1183
Film Propertiesdry / condUnitTest Standard
Stress at yield (parallel) 85 / * MPa ISO 527-3
Stress at yield (normal) 85 / * MPa ISO 527-3
Strain at yield (parallel) 5 / * % ISO 527-3
Strain at yield (normal) 5 / * % ISO 527-3
Maximum strain (parallel) 300 / * % ISO 527-3
Maximum strain (normal) 300 / * % ISO 527-3
Elmendorf Tear resistance (parallel) 10 / * N ISO 6383-2
Elmendorf Tear resistance (normal) 10 / * N ISO 6383-2
Trouser Tear resistance (parallel) 5 / * N/mm ISO 6383-1
Trouser Tear resistance (normal) 5 / * N/mm ISO 6383-1
Gloss, 60° 160 / * - ISO 2813
WVTR (23°C/85%r.h.) 7 / * g/(m²*d) DIS 15106-1/-2
Oxygen transmission rate (23°C/0%r.h.) 30 / * cm³/(m²*d*bar) DIS 15105-1/-2
Oxygen transmission rate (23°C/85%r.h.) 10 / * cm³/(m²*d*bar) DIS 15105-1/-2
Carbon Dioxide transm. rate (23°C/0%r.h.) 90 / * cm³/(m²*d*bar) DIS 15105-1/-2
Carbon Dioxide transm. rate (23°C/85%r.h.) 40 / * cm³/(m²*d*bar) DIS 15105-1/-2
Characteristics
Processing
Blow Molding
Delivery form
Pellets
Special Characteristics
Transparent
Regional Availability
Disclaimer
EMS-CHEMIE AG
Business Unit EMS-GRIVORY

Homepage : EMS-GRIVORY
eMail    : welcome@emsgrivory.com


In the line with the aims of CAMPUS, the values are intended to serve as
an aid in preselecting materials and  for an overview of the EMS-GRIVORY
product  range.  They  correspond  to our  current  knowledge,  a  legal
guarantee concerning the application and the manufacture can however not
be assumed.  This data does not  cancel the processor's  own testing and
inspection obligations.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991