CAMPUS® datasheet | HOSTAFORM C 9021 S1


This datasheet of HOSTAFORM C 9021 S1 from Ticona is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  HOSTAFORM C 9021 S1 | POM | Ticona
Product Texts
POM copolymer

Standard-Injection molding type with high rigidity, hardness and
toughness; good chemical resistance. Modified with 1% silicon oil
Available in natural and colored

Fulfils EG-directive 10/2011 as well as the recommendation
XXXIII for consumer goods of the BfR,
FDA compliant according to 21 CFR 177.2470

Burning rate ISO 3795 and FMVSS 302 < 100mm/min for a thickness more
than 1 mm.

Ranges of applications: precision engineering, electric and
electronical industry, domestic
appliances.

FDA = Food and Drug Administration (USA)
BfR = Bundesinstitut für Risikobewertung (Germany)
FMVSS = Federal Motor Vehicle Safety Standard (USA)
Rheological propertiesValueUnitTest Standard
Molding shrinkage (parallel) 2.0 % ISO 294-4, 2577
Molding shrinkage (normal) 1.8 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2700 MPa ISO 527-1/-2
Yield stress 60 MPa ISO 527-1/-2
Yield strain 11.5 % ISO 527-1/-2
Nominal strain at break 35 % ISO 527-1/-2
Charpy impact strength (+23°C) 180[P] kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 160 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6.5 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 6 kJ/m² ISO 179/1eA
P: Partial Break
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 166 °C ISO 11357-1/-3
Coeff. of linear therm. expansion (parallel) 110 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 110 E-6/K ISO 11359-1/-2
Other propertiesValueUnitTest Standard
Water absorption 0.65 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1410 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1200 kg/m³ -
Thermal conductivity of melt 0.155 W/(m K) -
Spec. heat capacity melt 2210 J/(kg K) -
Eff. thermal diffusivity 4.85E-8 m²/s -
Ejection temperature 165 °C -
Test specimen productionValueUnitTest Standard
Processing conditions acc. ISO 9990 - ISO ....-2
Injection Molding, melt temperature 205 °C ISO 294
Injection Molding, mold temperature 90 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Injection Molding, pressure at hold 90 MPa ISO 294
Diagrams
Specific volume-temperature (pvT) , HOSTAFORM C 9021 S1, POM, Ticona
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Sheet Extrusion, Other Extrusion, Blow Molding
Delivery form
Pellets
Additives
Release agent
Regional Availability
Disclaimer
NOTICE TO USERS: Values shown are based on testing
of laboratory test specimens and represent data that fall
within the standard range of properties for natural material.
These values alone do not represent a sufficient basis for
any part design and are not intended for use in
establishing maximum, minimum, or ranges of values for
specification purposes. Colorants or other additives may
cause significant variations in data values.

Properties of molded parts can be influenced by a wide
variety of factors including, but not limited to, material
selection, additives, part design, processing conditions and
environmental exposure. Any determination of the
suitability of a particular material and part design for any
use contemplated by the users and the manner of such
use is the sole responsibility of the users, who must assure
themselves that the material as subsequently processed
meets the needs of their particular product or use.

To the best of our knowledge, the information contained in
this publication is accurate; however, we do not assume
any liability whatsoever for the accuracy and completeness
of such information. The information contained in this
publication should not be construed as a promise or
guarantee of specific properties of our products. It is the
sole responsibility of the users to investigate whether any
existing patents are infringed by the use of the materials
mentioned in this publication.

Moreover, there is a need to reduce human exposure to
many materials to the lowest practical limits in view of
possible adverse effects. To the extent that any hazards
may have been mentioned in this publication, we neither
suggest nor guarantee that such hazards are the only ones
which exist. We recommend that persons intending to rely
on any recommendation or to use any equipment,
processing technique, or material mentioned in this
publication should satisfy themselves that they can meet
all applicable safety and health standards.

We strongly recommend that users seek and adhere to the
manufacturer's current instructions for handling each
material they use, and to entrust the handling of such
material to adequately trained personnel only. Please call
the telephone numbers listed for additional technical
information. Call Customer Services for the appropriate
Materials Safety Data Sheets (MSDS) before attempting to
process our products.

The products mentioned herein are not intended for use in
medical or dental implants.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991