offers extended functionality!CAMPUS® datasheet | HOSTAFORM LGC90-QX
This datasheet of HOSTAFORM LGC90-QX from Ticona is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
HOSTAFORM LGC90-QX | POM-GF26 | Ticona
Product Texts
Preliminary Data Sheet
Hostaform® LGC90-QX acetal copolymer is a specialty long fiber glass
coupled grade formulated to provide exceptional mechanical properties
while retaining other properties typical of acetal copolymers such as
inherent lubricity and chemical resistance.
LGC90-QX is supplied in pellet form and is suitable for injection,
injection-compression, extrusion, and extrusion-compression processes.
For important additional process or equipment recommendations, please
reference www.ticona.com/tech/processing under Celstran LFRT and Compel
LFRT, or call the Ticona product hotline to request further information.
Hostaform® LGC90-QX acetal copolymer is a specialty long fiber glass
coupled grade formulated to provide exceptional mechanical properties
while retaining other properties typical of acetal copolymers such as
inherent lubricity and chemical resistance.
LGC90-QX is supplied in pellet form and is suitable for injection,
injection-compression, extrusion, and extrusion-compression processes.
For important additional process or equipment recommendations, please
reference www.ticona.com/tech/processing under Celstran LFRT and Compel
LFRT, or call the Ticona product hotline to request further information.
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 9500 | MPa | ISO 527-1/-2 |
| Stress at break | 160 | MPa | ISO 527-1/-2 |
| Strain at break | 2.6 | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | 60 | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 26 | kJ/m² | ISO 179/1eA |
| Thermal properties | Value | Unit | Test Standard |
| Melting temperature (10°C/min) | 167 | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 166 | °C | ISO 75-1/-2 |
| Other properties | Value | Unit | Test Standard |
| Density | 1600 | kg/m³ | ISO 1183 |
Characteristics
Processing
Injection Molding, Profile Extrusion, Sheet Extrusion
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Predrying is not required unless material came in contact with
significant moisture.
PROCESSING
Long Fiber Reinforced Thermoplastic products may be processed using
current standard injection molding machines having screw diameters
greater than 40mm (1.6 inches).
A three-zone screw should be used, having a feed zone of approximately
ten diameters, a compression zone of six, and a metering zone of four
diameters. It should have an L/D ratio of 20:1 with a compression
ratio of about 2:1. Screw flight depth should be at least 4.5mm (0.18
inches).
Wear and corrosion protective measures are recommended. Use interior
armouring or a bimetallic coating on the cylinder and arm parts of the
non-return valve with powdered metal steels. Additional corrosion
protection of the melt carrying components in the plastication unit is
recommended when working with Celstran LFRT nylon or PPS produ cts.
Due to the short residence time, suitable shot volumes are from 30% to
70 % of the maximum metering capacity of the machine.
LFRT is usually processed using a free flow nozzle, but it requires an
orifice diameter greater than 0.16 inches (4 mm) and preferably larger
than 0.125 inches (6 mm). A shut-off nozzle may be advisable if a
large orifice is used. An easy flowing, three-part, check-ring type of
non-return valve with a large cross section is recommended.
POSTPROCESSING
Predrying is not required unless material came in contact with
significant moisture.
PROCESSING
Long Fiber Reinforced Thermoplastic products may be processed using
current standard injection molding machines having screw diameters
greater than 40mm (1.6 inches).
A three-zone screw should be used, having a feed zone of approximately
ten diameters, a compression zone of six, and a metering zone of four
diameters. It should have an L/D ratio of 20:1 with a compression
ratio of about 2:1. Screw flight depth should be at least 4.5mm (0.18
inches).
Wear and corrosion protective measures are recommended. Use interior
armouring or a bimetallic coating on the cylinder and arm parts of the
non-return valve with powdered metal steels. Additional corrosion
protection of the melt carrying components in the plastication unit is
recommended when working with Celstran LFRT nylon or PPS produ cts.
Due to the short residence time, suitable shot volumes are from 30% to
70 % of the maximum metering capacity of the machine.
LFRT is usually processed using a free flow nozzle, but it requires an
orifice diameter greater than 0.16 inches (4 mm) and preferably larger
than 0.125 inches (6 mm). A shut-off nozzle may be advisable if a
large orifice is used. An easy flowing, three-part, check-ring type of
non-return valve with a large cross section is recommended.
POSTPROCESSING
Disclaimer
NOTICE TO USERS: Values shown are based on testing of laboratory test specimens and represent data that fall within the standard range of properties for natural material. These values alone do not represent a sufficient basis for any part design and are not intended for use in establishing maximum, minimum, or ranges of values for specification purposes. Colorants or other additives may cause significant variations in data values. Properties of molded parts can be influenced by a wide variety of factors including, but not limited to, material selection, additives, part design, processing conditions and environmental exposure. Any determination of the suitability of a particular material and part design for any use contemplated by the users and the manner of such use is the sole responsibility of the users, who must assure themselves that the material as subsequently processed meets the needs of their particular product or use. To the best of our knowledge, the information contained in this publication is accurate; however, we do not assume any liability whatsoever for the accuracy and completeness of such information. The information contained in this publication should not be construed as a promise or guarantee of specific properties of our products. It is the sole responsibility of the users to investigate whether any existing patents are infringed by the use of the materials mentioned in this publication. Moreover, there is a need to reduce human exposure to many materials to the lowest practical limits in view of possible adverse effects. To the extent that any hazards may have been mentioned in this publication, we neither suggest nor guarantee that such hazards are the only ones which exist. We recommend that persons intending to rely on any recommendation or to use any equipment, processing technique, or material mentioned in this publication should satisfy themselves that they can meet all applicable safety and health standards. We strongly recommend that users seek and adhere to the manufacturer's current instructions for handling each material they use, and to entrust the handling of such material to adequately trained personnel only. Please call the telephone numbers listed for additional technical information. Call Customer Services for the appropriate Materials Safety Data Sheets (MSDS) before attempting to process our products. The products mentioned herein are not intended for use in medical or dental implants.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991