View list of
  • All ARKEMA grades
  • All PVDF grades
  • All grades beginning with K

CAMPUS® datasheet | KYNAR 9000 HDC N 123


This datasheet of KYNAR 9000 HDC N 123 from ARKEMA is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  KYNAR 9000 HDC N 123 | PVDF-CF... | ARKEMA
Product Texts
DESIGNATION ISO 12086-PVDF-E,GG1,Q.5E5.J.A.I.D, CF,

KYNAR PVDF are fluorinated thermoplastic homopolymers.


Outstanding characteristics of KYNAR : chemical resistance, imperviousness 
to UV, high barrier properties, high purity, good mechanical and 
thermomechanical properties.

Main applications of KYNAR: corrosion protection in the chemical industry, 
coating (painting, coextrusion), off shore, wire and cable.

KYNAR 9000 HDC N 123 is a high stiffness carbon fiber filled grade of 
granules.
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 2.4 cm³/10min ISO 1133
Temperature 230 °C ISO 1133
Load 5 kg ISO 1133
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 7000 MPa ISO 527-1/-2
Stress at break 70 MPa ISO 527-1/-2
Strain at break 2 % ISO 527-1/-2
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 170 °C ISO 11357-1/-3
Glass transition temperature (10°C/min) -42 °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 125 °C ISO 75-1/-2
Burning Behav. at 1.5 mm nom. thickn. V-0 class IEC 60695-11-10
Thickness tested 1.6 mm IEC 60695-11-10
Burning Behav. at thickness h V-0 class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
Other propertiesValueUnitTest Standard
Water absorption 0.15 % Sim. to ISO 62
Humidity absorption 0.015 % Sim. to ISO 62
Density 1800 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 220 °C ISO 294
Injection Molding, mold temperature 90 °C ISO 10724
Injection Molding, injection velocity 10 mm/s ISO 294
Injection Molding, pressure at hold 13 MPa ISO 294
Diagrams
Viscosity-shear rate , KYNAR 9000 HDC N 123, PVDF-CF..., ARKEMA
Shearstress-shear rate , KYNAR 9000 HDC N 123, PVDF-CF..., ARKEMA
Stress-strain , KYNAR 9000 HDC N 123, PVDF-CF..., ARKEMA
Secant modulus-strain , KYNAR 9000 HDC N 123, PVDF-CF..., ARKEMA
Characteristics
Processing
Injection Molding
Delivery form
Granules
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PROCESSING
     

Melt temperature :      220-240 °C
Mold temperature :       70- 90 °C

Notice text      :      Due to the important shrinkage it is necessary to  
                 :      adapt thepressure keeping time in the mold.

                 :      Example of a 52 seconds cycle

                 :      - injection      : 10 s - keeping : 20 s
                 :      - plastification : 15 s - waiting :  7 s

POSTPROCESSING


Annealing              
-Temperature     :      150     °C
-Time            :      1       h
Chemical Media Resistance
Acids
Acetic Acid (5% by mass) (23°C)
Citric Acid solution (10% by mass) (23°C)
Lactic Acid (10% by mass) (23°C)
Hydrochloric Acid (36% by mass) (23°C)
Nitric Acid (40% by mass) (23°C)
Sulfuric Acid (38% by mass) (23°C)
Sulfuric Acid (5% by mass) (23°C)
Chromic Acid solution (40% by mass) (23°C)
Bases
Sodium Hydroxide solution (35% by mass) (23°C)
Sodium Hydroxide solution (1% by mass) (23°C)
Ammonium Hydroxide solution (10% by mass) (23°C)
Alcohols
Isopropyl alcohol (23°C)
Methanol (23°C)
Ethanol (23°C)
Hydrocarbons
n-Hexane (23°C)
Toluene (23°C)
iso-Octane (23°C)
Ketones
Acetone (23°C)
Ethers
Diethyl ether (23°C)
Mineral oils
SAE 10W40 multigrade motor oil (23°C)
SAE 10W40 multigrade motor oil (130°C)
SAE 80/90 hypoid-gear oil (130°C)
Insulating Oil (23°C)
Standard Fuels
ISO 1817 Liquid 1 (60°C)
ISO 1817 Liquid 2 (60°C)
ISO 1817 Liquid 3 (60°C)
ISO 1817 Liquid 4 (60°C)
Standard fuel without alcohol (pref. ISO 1817 Liquid C) (23°C)
Standard fuel with alcohol (pref. ISO 1817 Liquid 4) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (23°C)
Diesel fuel (pref. ISO 1817 Liquid F) (90°C)
Diesel fuel (pref. ISO 1817 Liquid F) (>90°C)
Salt solutions
Sodium Chloride solution (10% by mass) (23°C)
Sodium Hypochlorite solution (10% by mass) (23°C)
Sodium Carbonate solution (20% by mass) (23°C)
Sodium Carbonate solution (2% by mass) (23°C)
Zinc Chloride solution (50% by mass) (23°C)
Other
Ethyl Acetate (23°C)
Hydrogen peroxide (23°C)
Ethylene Glycol (50% by mass) in water (108°C)
Water (23°C)
Deionized water (90°C)
Phenol solution (5% by mass) (23°C)
Disclaimer

This database provides the main properties of technical thermoplastics
marketed by ARKEMA.

      The information contained in this document is based on trials carried
out by our Research Centres and data selected from the literature, but
shall in no event be held to constitute or imply any warranty,
undertaking, express or implied commitment from our part.
Our format specifications define the limit of our commitment.
No liability whatsoever can be accepted by ARKEMA with regard to the
handling processing or use of the product or products concerned which
much in all cases be employed in accordance with all relevant laws
and/or regulations in force in the country or countries concerned.

For information about the other products marketed
by our company consult :
ARKEMAGROUP.COM

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991