  LAURAMID® B | PA12 | Evonik Industries AG
Product Texts
LAURAMID® B

 

Resin: DIN-16880-PA 12G

 

LAURAMID®  is a polyamide 12 produced from laurinlactam by the lactam
casting method. The low viscosity melt fills the mold without pressure and
is polymerized in the mold. This procedure excludes the use of regenerated
material.


The test bars were prepared by machining from cast plaques.
LAURAMID® molded materials, profiles, ready made parts and Systems were
prepared by:
Albert Handtmann ELTEKA GmbH & Co. KG.
Every delivered part from A.Handmann is checked by X-ray diagnosis.
LAURAMID® B exhibits, due to its very low water absorption, very good
hydrolysis resistance: good dimensional stability, tear resistance and
chemical resistance as well as an outstanding creep resistance.

 

Application examples: Cogs, sprockets and spiral drive wheels, 

                                    rollers, propellers, cleaner parts, pump parts.

Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2100 MPa ISO 527-1/-2
Yield stress 60 MPa ISO 527-1/-2
Yield strain 8 % ISO 527-1/-2
Nominal strain at break 18 % ISO 527-1/-2
Charpy impact strength (+23°C) 175 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 85 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 4 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Temp. of deflection under load (1.80 MPa) 190 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 194 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 188 °C ISO 306
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.5 - IEC 60250
Dissipation factor (100Hz) 380 E-4 IEC 60250
Volume resistivity 1E12 Ohm*m IEC 60093
Surface resistivity 1E14 Ohm IEC 60093
Other propertiesValueUnitTest Standard
Water absorption 1.4 % Sim. to ISO 62
Humidity absorption 0.9 % Sim. to ISO 62
Density 1030 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, pressure at hold 70 MPa ISO 294
Diagrams
Stress-strain , LAURAMID® B, PA12, Evonik Degussa
Secant modulus-strain , LAURAMID® B, PA12, Evonik Degussa
Characteristics
Processing
Casting
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Disclaimer
With the following data, which reflect our current knowledge and experience,
we wish to describe possible applications, however this information is given
without guarantee or assurance of the appropriate properties for a specific
application.

The processor is not relieved of the responsibility for incoming quality control
nor from his own testing and analysis.

All data concerning product safety (EG-guideline, BGVV, FDA) are of principle
nature and can be limitied regarding migration, temperature and type of food.
They reflect the status as of Feb. 29, 2012. To insure that this data reflects the
current state, please contact our Product Safety Department.

Should you have any questions, wishes or suggestions about CAMPUS,
please refer to the following address:

  Link to Evonik Industries AG homepage

In any case, we hope you enjoy working with CAMPUS!

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991