CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
- ISO 7391-PC,MFR,(,,)-05-3,GF20
- Global grade
- MVR (300 °C/1.2 kg) 5.0 cm3/10 min
- 20 % Glass fiber reinforced
- Chlorine- and bromine-free flame retardant
- UL 94V-0/1.5 mm and 5VA/3.0 mm
- High viscosity
- Easy release
- Extrusion
- Injection molding - Melt temperature 310 - 330 °C
- Available in opaque colors only
| Rheological properties | Value | Unit | Test Standard |
| Melt volume-flow rate (MVR) | 5 | cm³/10min | ISO 1133 |
| Temperature | 300 | °C | ISO 1133 |
| Load | 1.2 | kg | ISO 1133 |
| Molding shrinkage (parallel) | 0.3 | % | ISO 294-4, 2577 |
| Molding shrinkage (normal) | 0.5 | % | ISO 294-4, 2577 |
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 5800 | MPa | ISO 527-1/-2 |
| Stress at break | 85 | MPa | ISO 527-1/-2 |
| Strain at break | 2.6 | % | ISO 527-1/-2 |
| Tensile creep modulus (1h) | 5700 | MPa | ISO 899-1 |
| Tensile creep modulus (1000h) | 5200 | MPa | ISO 899-1 |
| Charpy impact strength (+23°C) | 40 | kJ/m² | ISO 179/1eU |
| Charpy impact strength (-30°C) | 50 | kJ/m² | ISO 179/1eU |
| Puncture - maximum force (+23°C) | 900 | N | ISO 6603-2 |
| Puncture - maximum force (-30°C) | 900 | N | ISO 6603-2 |
| Puncture energy (+23°C) | 5 | J | ISO 6603-2 |
| Puncture energy (-30°C) | 5 | J | ISO 6603-2 |
| Thermal properties | Value | Unit | Test Standard |
| Temp. of deflection under load (1.80 MPa) | 138 | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 142 | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 147 | °C | ISO 306 |
| Coeff. of linear therm. expansion (parallel) | 30 | E-6/K | ISO 11359-1/-2 |
| Coeff. of linear therm. expansion (normal) | 65 | E-6/K | ISO 11359-1/-2 |
| Burning Behav. at 1.5 mm nom. thickn. | V-0 | class | IEC 60695-11-10 |
| Thickness tested | 1.5 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Burning Behav. at thickness h | V-0 | class | IEC 60695-11-10 |
| Thickness tested | 3.0 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Burning Behav. 5V at thickness h | 5VA | class | IEC 60695-11-20 |
| Thickness tested | 3.0 | mm | IEC 60695-11-20 |
| UL recognition | UL | - | - |
| Oxygen index | 35 | % | ISO 4589-1/-2 |
| Electrical properties | Value | Unit | Test Standard |
| Relative permittivity (100Hz) | 3.3 | - | IEC 60250 |
| Relative permittivity (1MHz) | 3.3 | - | IEC 60250 |
| Dissipation factor (100Hz) | 10 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | 90 | E-4 | IEC 60250 |
| Volume resistivity | >1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | >1E15 | Ohm | IEC 60093 |
| Electric strength | 36 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 175 | - | IEC 60112 |
| Other properties | Value | Unit | Test Standard |
| Water absorption | 0.24 | % | Sim. to ISO 62 |
| Humidity absorption | 0.1 | % | Sim. to ISO 62 |
| Density | 1340 | kg/m³ | ISO 1183 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Density of melt | 1140 | kg/m³ | - |
| Thermal conductivity of melt | 0.255 | W/(m K) | - |
| Spec. heat capacity melt | 1820 | J/(kg K) | - |
| Eff. thermal diffusivity | 1.23E-7 | m²/s | - |
| Ejection temperature | 140 | °C | - |
| Test specimen production | Value | Unit | Test Standard |
| Processing conditions acc. ISO | 7390 | - | ISO ....-2 |
| Injection Molding, melt temperature | 300 | °C | ISO 294 |
| Injection Molding, mold temperature | 110 | °C | ISO 10724 |
| Injection Molding, injection velocity | 200 | mm/s | ISO 294 |
| Injection Molding, pressure at hold | 500 | MPa | ISO 294 |
Preprocessing
| Max. Water content | 0.02 % |
| Drying temperature | 120 °C |
| Drying time | |
| Circulating air drying oven (50 % fresh air) | 4-12 h |
| Fresh air dryer (high speed dryer) | 2-4 h |
| Dry air dryer | 2-3 h |
Process ing
| Melt temperature | 310-330 °C |
| Mold temperature | 80-130 °C |
Preprocessing
| Max. Water content | 0.01 % |
| Drying temperature | 120 °C |
| Drying time | |
| Circulating air drying oven (50 % fresh air) | 4-12 h |
| Fresh air dryer (high speed dryer) | 2-4 h |
| Dry air dryer | 2-3 h |
Process ing
| Melt temperature | 230-280 °C |
Bayer MaterialScience AG
This information and our technical advice - whether verbal, in writing or by way of trials - are given in good faith but without warranty, and this also applies where proprietary rights of third parties are involved. Our advice does not release you from the obligation to check its validity and to test our products as to their suitability for the intended processes and uses. The application, use and processing of our products and the products manufactured by you on the basis of our technical advice are beyond our control and, therefore, entirely your own responsibility. Our products are sold in accordance with our General Conditions of and Delivery. The values stored in the databank should only be used as guidelines for component design. In giving these values neither guarantee, nor assurance of particular material properties can be given.
Bayer MaterialScience LLC - CAMPUS version 5.x
This database, the data, reports, and graphs generated by the software [as of March 2010] have been provided pursuant to an agreement containing restrictions of their use between Bayer and Wirtschaftsförderungs-Gesellschaft CWF GmbH, Frankfurt am Main, Germany. They are also protected by Copyright and cannot be copied, or distributed, transmitted, transcribed, or translated into any human or computer language, in any form or by any means without the expressed written consent of Bayer Materialscience LLC, Pittsburgh, Pa. 15205-9741.
DISCLAIMER OF ALL WARRANTIES AND LIMITATION OF LIABILITY
BAYER MATERIALSCIENCE LLC DISCLAIMS ALL WARRANTIES WITH REGARD TO THIS SOFTWARE, INCLUDING ALL IMPLIED WARRANTIES OF MERCHANTABILITY AND FITNESS FOR A PARTICULAR PURPOSE. IN NO EVENT SHALL BAYER MATERIALSCIENCE LLC BE LIABLE FOR ANY DAMAGES WHATSOEVER OF WHATEVER NATURE, WHETHER DIRECT, SPECIAL, INDIRECT, INCIDENTAL, OR CONSEQUENTIAL, ARISING FROM BREACH OF CONTRACT OR WARRANTY, NEGLIGENCE, OR ANY OTHER ACT, AND WHICH ARISE OUT OF OR IN CONNECTION WITH THE USE OR PERFORMANCE OF THIS SOFTWARE.
Bayer MaterialScience LLC - Standard Disclaimer
The manner in which you use and the purpose to which you put and utilize our products, technical assistance and information (whether verbal, written or by way of production evaluations), including any suggested formulations and recommendations are beyond our control. Therefore, it is imperative that you test our products, technical assistance and information to determine to your own satisfaction whether they are suitable for your intended uses and applications. This application-specific analysis must at least include testing to determine suitability from a technical as well as health, safety, and environmental. Such testing has not necessarily been done by us. Unless we otherwise agree in writing, all products are sold strictly pursuant to the terms of our standard conditions of sale. All information and technical assistance is given without warranty or guarantee and is subject to change without notice. It is expressly understood and agreed that you assume and hereby expressly release us from all liability, in tort, contract or otherwise, incurred in connection with the use of our products, technical assistance, and information. Any statement or recommendation not contained herein is unauthorized and shall not bind us. Nothing herein shall be construed as a recommendation to use any product in conflict with patents covering any material or its use. No license is implied or in fact granted under the claims of any patent.
www.bayerplastics.comCAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991