View list of

CAMPUS® datasheet | PLEXIGLAS® Satinice df22 zk6BR


This datasheet of PLEXIGLAS® Satinice df22 zk6BR from Evonik Röhm GmbH is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  PLEXIGLAS® Satinice df22 zk6BR | PMMA | Evonik Röhm GmbH
Product Texts

Productprofil:

PLEXIGLAS® Satinice df22 zk6BR, based on PLEXIGLAS® Resist zk6BR, is an impact modified molding compound characterized by diffuse scattering of light.

 

Typical properties of impact modified PLEXIGLAS® molding compound are

 

  • high break resistance and impact strength
  • improved resistance to stress cracking
  • good weather resistance
  • high surface hardness and mar resistance
  • the pleasant feel and sound of the moldings.

 

PLEXIGLAS® Satinice df22 zk6BR is characterized by the following special properties:

 

  • very good lightdiffusion combined with excellent light transmission
  • matte surfaces can be obtained by varying the extrusion parameters.

Application:

Used for extruding profiles and sheets, but also for injection molding items for lighting engineering applications

Example:

applications that call for light diffusion combined with optimum transmission

Processing:

PLEXIGLAS® Satinice df22 zk6BR can be processed on extruders with 3-zone general purpose screws for engineering thermoplastics.

The matte finish of profile surfaces depends very much on machine design (calibrating unit, polishing rolls) and cooling conditions. It can be enhanced by controlled temperature reduction.

Physical Form / Packaging:

PLEXIGLAS® Satinice df molding compounds are supplied as pellets of uniform size, packaged in 25kg polyethylene bags; other packaging on request.

Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 1.4 cm³/10min ISO 1133
Temperature 230 °C ISO 1133
Load 3.8 kg ISO 1133
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 1800 MPa ISO 527-1/-2
Yield stress 45 MPa ISO 527-1/-2
Yield strain 5 % ISO 527-1/-2
Nominal strain at break 40 % ISO 527-1/-2
Charpy impact strength (+23°C) 54 kJ/m² ISO 179/1eU
Thermal propertiesValueUnitTest Standard
Glass transition temperature (10°C/min) 109 °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 93 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 99 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 98 °C ISO 306
Coeff. of linear therm. expansion (parallel) 90 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Electrical propertiesValueUnitTest Standard
Volume resistivity >1E13 Ohm*m IEC 60093
Surface resistivity 1E13 Ohm IEC 60093
Other propertiesValueUnitTest Standard
Density 1150 kg/m³ ISO 1183
Material specific propertiesValueUnitTest Standard
Luminous transmittance 86 % ISO 13468-1, -2
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 255 °C ISO 294
Injection Molding, mold temperature 58 °C ISO 10724
Injection Molding, injection velocity 195 mm/s ISO 294
Diagrams
Viscosity-shear rate , PLEXIGLAS® Satinice df22 zk6BR, PMMA, Evonik Röhm
Shearstress-shear rate , PLEXIGLAS® Satinice df22 zk6BR, PMMA, Evonik Röhm
Dynamic Shear modulus-temperature , PLEXIGLAS® Satinice df22 zk6BR, PMMA, Evonik Röhm
Stress-strain , PLEXIGLAS® Satinice df22 zk6BR, PMMA, Evonik Röhm
Secant modulus-strain , PLEXIGLAS® Satinice df22 zk6BR, PMMA, Evonik Röhm
Tensile modulus-temperature , PLEXIGLAS® Satinice df22 zk6BR, PMMA, Evonik Röhm
Characteristics
Processing
Injection Molding, Profile Extrusion, Sheet Extrusion, Other Extrusion
Delivery form
Pellets
Additives
Release agent
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather
Regional Availability
Other text information
Injection molding
PREPROCESSING
Predrying temperature: max. 80 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Min. melt temperature: 220 - 260°C
Min. mold temperature:60 - 90°C
Profile extrusion
PREPROCESSING
Predrying temperature: max. 80 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 230 - 260 °C

Die temperature: 230 - 260 °C
Sheet extrusion
PREPROCESSING
Predrying temperature: max. 80 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 230 - 260 °C
Die temperature: 230 - 260 °C
Disclaimer
All listed technical data are typical values intended for your
guidance. They are given without obligation and do not constitute a
materials specification. Should you have any further questions
concerning material behavior or properties, please contact us
at the following address :

                     Evonik Röhm GmbH
                     Marketing / Campus
                     Kirschenallee
                     D-64293 Darmstadt
                     Germany
                     Phone: +49 - (0) 61 51 / 18-47 11
                     Fax:   +49 - (0) 61 51 / 18-31 77
                     E-Mail: campusplastics@evonik.com
                     Internet: http://www.plexiglas.net

® = registered trademark

PLEXIGLAS® is a registered trademark of Evonik Röhm GmbH, Germany,
outside of the Americas. Within the Americas it is sold as ACRYLITE®,
which is a registered trademark of Evonik Cyro LLC, USA.
PLEXIMID® is a registered trademarks of Evonik Röhm GmbH, Germany.
CYROLITE® and XT® polymer are registered trademarks of Evonik Cyro LLC, USA. 

This information and all further technical advice is based on our present knowledge

and experience. However, it implies no liability or other legal responsibility on our part,

including with regard to existing third party intellectual property rights, especially

patent rights. In particular, no warranty, whether express or implied, or guarantee of

product properties in the legal sense is intended or implied. We reserve the right to

make any changes according to technological progress or further developments. The

customer is not released from the obligation to conduct careful inspection and testing

of incoming goods. Performance of the product described herein should be verified by

testing, which should be carried out only by qualified experts in the sole responsibility

of a customer. Reference to trade names used by other companies is neither a

recommendation, nor does it imply that similar products could not be used.

 

NAFTA:

This information and all technical and other advice are based on Evonik’s

present knowledge and experience. However, Evonik assumes no liability for

such information or advice, including the extent to which such information or

advice may relate to third party intellectual property rights. Evonik reserves the

right to make any changes to information or advice at any time, without prior

or subsequent notice. EVONIK DISCLAIMS ALL REPRESENTATIONS AND

WARRANTIES, WHETHER EXPRESS OR IMPLIED, AND SHALL HAVE NO LIABILITY

FOR, MERCHANTABILITY OF THE PRODUCT OR ITS FITNESS FOR A PARTICULAR

PURPOSE (EVEN IF EVONIK IS AWARE OF SUCH PURPOSE), OR OTHERWISE.

EVONIK SHALL NOT BE RESPONSIBLE FOR CONSEQUENTIAL, INDIRECT OR

INCIDENTAL DAMAGES (INCLUDING LOSS OF PROFITS) OF ANY KIND. It is the

customer’s sole responsibility to arrange for inspection and testing of all

products by qualified experts. Reference to trade names used by other

companies is neither a recommendation nor an endorsement of the

corresponding product, and does not imply that similar products could not be

used.

Sales range and technical data subject to alteration.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991