  RADIFLAM® B RV250AE | PBT-GF25 FR | RadiciPlastics
Product Texts
DESIGNATION:
Thermoplastics ISO 7792-PBT, MFGRS, 09-080, GF25

BRIEF DESCRIPTION:
PBT Flame retardant injection moulding grade
25% Glass fibre reinforced.
For high stiffness components.
UL94 V0 rated at 0,8mm
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 10100 MPa ISO 527-1/-2
Stress at break 95 MPa ISO 527-1/-2
Strain at break 1.4 % ISO 527-1/-2
Charpy impact strength (+23°C) 26 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 23 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6.6 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 6 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 225 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 195 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 205 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 205 °C ISO 306
Burning Behav. at 1.5 mm nom. thickn. V-0 class IEC 60695-11-10
Thickness tested 1.6 mm IEC 60695-11-10
UL recognition UL - -
Burning Behav. at thickness h V-0 class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
UL recognition UL - -
Electrical propertiesValueUnitTest Standard
Volume resistivity 1E13 Ohm*m IEC 60093
Comparative tracking index 250 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.3 % Sim. to ISO 62
Humidity absorption 0.1 % Sim. to ISO 62
Density 1620 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Processing conditions acc. ISO 7792 - ISO ....-2
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre-drying recommended.
Max. water content 0.04%
Drying temperature 110°C
Drying time 2-4h (dry air dryer)
PROCESSING
Melt temperature 260°C
Mold temperature 80°C
Disclaimer
This database provides the technical properties
of thermoplastics produced and marketed by
RADICI NOVACIPS
and his subsidiaries companies:

RADILON® A          Polyamide 66
RADILON® S          Polyamide 6
RADILON® CA       Copolyamide 66/6
RADILON® CS       Copolyamide 6 semiaromatic
RADITER® B          Poly(butylene terephthalate)
RADIFLAM® A         Polyamide 66,  self-extinguishing
RADIFLAM® S         Polyamide 6,   self-extinguishing
RADIFLAM® B         Polybutylene terephthalate, self-extinguishing
HERAFLEX® A        Stirenic Thermoplastic Elastomer SEBS
HERAFLEX® E        Ether-Ester Thermoplastic Elastomer
HERAFLEX® B        Stirenic Thermoplastic Elastomer SBS
HERAFLEX® P        Modified Polypropylene
RADILENE® R        Polyethylene and Polypropylene

The data and graphs contained in this database were carried out
by our Research Centers and shall in no event be held to
constitute or imply any warranty, undertaking, express or
implied commitment from our part.

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991