This datasheet of RADILON® A RV250 from RadiciPlastics is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
RADILON® A RV250 | PA66-GF25 | RadiciPlastics
Product Texts
DESIGNATION:
Thermoplastics ISO1874-PA66,MR,14-090,GF25
BRIEF DESCRIPTION:
PA66 25% Glass fibre reinforced injection moulding grade.
For items with medium stiffness.
Thermoplastics ISO1874-PA66,MR,14-090,GF25
BRIEF DESCRIPTION:
PA66 25% Glass fibre reinforced injection moulding grade.
For items with medium stiffness.
| Mechanical properties | dry / cond | Unit | Test Standard |
| Tensile Modulus | 8300 / 6500 | MPa | ISO 527-1/-2 |
| Stress at break | 160 / 110 | MPa | ISO 527-1/-2 |
| Strain at break | 3.6 / 3.8 | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | 61 / - | kJ/m² | ISO 179/1eU |
| Charpy impact strength (-30°C) | 57 / - | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 12 / - | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | 9.5 / - | kJ/m² | ISO 179/1eA |
| Thermal properties | dry / cond | Unit | Test Standard |
| Melting temperature (10°C/min) | 260 / * | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 225 / * | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 250 / * | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 245 / * | °C | ISO 306 |
| Burning Behav. at 1.5 mm nom. thickn. | HB / * | class | IEC 60695-11-10 |
| Thickness tested | 1.6 / * | mm | IEC 60695-11-10 |
| UL recognition | UL / * | - | - |
| Burning Behav. at thickness h | HB / * | class | IEC 60695-11-10 |
| Thickness tested | 0.8 / * | mm | IEC 60695-11-10 |
| UL recognition | UL / * | - | - |
| Electrical properties | dry / cond | Unit | Test Standard |
| Volume resistivity | >1E13 / 1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | * / 1E14 | Ohm | IEC 60093 |
| Comparative tracking index | * / 550 | - | IEC 60112 |
| Other properties | dry / cond | Unit | Test Standard |
| Water absorption | 7.4 / * | % | Sim. to ISO 62 |
| Humidity absorption | 2 / * | % | Sim. to ISO 62 |
| Density | 1300 / * | kg/m³ | ISO 1183 |
| Material specific properties | dry / cond | Unit | Test Standard |
| Viscosity number | 145 / * | cm³/g | ISO 307, 1157, 1628 |
| Test specimen production | Value | Unit | Test Standard |
| Processing conditions acc. ISO | 1874 | - | ISO ....-2 |
| Injection Molding, melt temperature | 290 | °C | ISO 294 |
| Injection Molding, mold temperature | 80 | °C | ISO 10724 |
Diagrams
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Lubricants
Regional Availability
Other text information
Injection molding
PREPROCESSING
Max. water content 0.2%
Drying temperature 80°C
Drying time 2-4h (dry air dryer)
PROCESSING
Melt temperature 290°C
Mold temperature 80°C
Max. water content 0.2%
Drying temperature 80°C
Drying time 2-4h (dry air dryer)
PROCESSING
Melt temperature 290°C
Mold temperature 80°C
Disclaimer
This database provides the technical properties of thermoplastics produced and marketed by RADICI NOVACIPS and his subsidiaries companies: RADILON® A Polyamide 66 RADILON® S Polyamide 6 RADILON® CA Copolyamide 66/6 RADILON® CS Copolyamide 6 semiaromatic RADITER® B Poly(butylene terephthalate) RADIFLAM® A Polyamide 66, self-extinguishing RADIFLAM® S Polyamide 6, self-extinguishing RADIFLAM® B Polybutylene terephthalate, self-extinguishing HERAFLEX® A Stirenic Thermoplastic Elastomer SEBS HERAFLEX® E Ether-Ester Thermoplastic Elastomer HERAFLEX® B Stirenic Thermoplastic Elastomer SBS HERAFLEX® P Modified Polypropylene RADILENE® R Polyethylene and Polypropylene The data and graphs contained in this database were carried out by our Research Centers and shall in no event be held to constitute or imply any warranty, undertaking, express or implied commitment from our part.
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.