  RILSAN AECN O TL | PA12 | ARKEMA
Product Texts
DESIGNATION ISO 1874-PA12,KHL,14-010
 RILSAN
 Extrusion grade for the sheathing of wires and cables. 
 Available colours : natural. 
 Heat and light stabilized.

 Low melt viscosity.

 High speed extrusion.
 Very good ability to be processed in thin wall thickness.
 Easy to colour.

 Example applications : Coating of cables with fine-gauge, telephone 
 cables, loose tube for optical fibers. 
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 1650 / 1400 MPa ISO 527-1/-2
Yield stress 51 / 41 MPa ISO 527-1/-2
Yield strain 5 / 15 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) - / N kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) - / N kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) - / 6 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) - / 6 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 178 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 55 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 135 / * °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 142 / * °C ISO 306
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Burning Behav. at thickness h V-2 / * class IEC 60695-11-10
Thickness tested 3.2 / * mm IEC 60695-11-10
Oxygen index 22 / * % ISO 4589-1/-2
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 3 / - - IEC 60250
Relative permittivity (1MHz) 3 / - - IEC 60250
Dissipation factor (100Hz) 634 / - E-4 IEC 60250
Dissipation factor (1MHz) 295 / - E-4 IEC 60250
Volume resistivity - / 1E12 Ohm*m IEC 60093
Surface resistivity * / 1E14 Ohm IEC 60093
Electric strength 29 / 30 kV/mm IEC 60243-1
Comparative tracking index * / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 1.6 / * % Sim. to ISO 62
Density 1010 / 1010 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 50 °C ISO 10724
Injection Molding, pressure at hold 16 MPa ISO 294
Diagrams
Viscosity-shear rate , RILSAN AECN O TL, PA12, ARKEMA
Shearstress-shear rate , RILSAN AECN O TL, PA12, ARKEMA
Stress-strain , RILSAN AECN O TL, PA12, ARKEMA
Secant modulus-strain , RILSAN AECN O TL, PA12, ARKEMA
Characteristics
Processing
Injection Molding, Other Extrusion, Coating
Delivery form
Pellets
Additives
Lubricants
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Other extrusion

PREPROCESSING

Max water content: < 0.1  %

Notice text      :      RILSAN is delivered in sealed bags and is
                 :      ready for use.

                 :      Every opened bag of RILSAN which has not been
                 :      used within two hours must, as a precaution, be
                 :      re-dried.
                  
                 :      Drying conditions are 4 h at 80-90 °C in a
                 :      forced-air oven.

PROCESSING

Melt temperature : 190 - 250 °C
Profile extrusion

PREPROCESSING

Max water content: < 0.1  %

Notice text      :      RILSAN is delivered in sealed bags and is
                 :      ready for use.

                 :      Every opened bag of RILSAN which has not been
                 :      used within two hours must, as a precaution, be
                 :      re-dried.
                  
                 :      Drying conditions are 4 h at 80-90 °C in a
                 :      forced-air oven.

PROCESSING

Melt temperature : 190 - 250 °C
Disclaimer

This database provides the main properties of technical thermoplastics
marketed by ARKEMA.

      The information contained in this document is based on trials carried
out by our Research Centres and data selected from the literature, but
shall in no event be held to constitute or imply any warranty,
undertaking, express or implied commitment from our part.
Our format specifications define the limit of our commitment.
No liability whatsoever can be accepted by ARKEMA with regard to the
handling processing or use of the product or products concerned which
much in all cases be employed in accordance with all relevant laws
and/or regulations in force in the country or countries concerned.

For information about the other products marketed
by our company consult :
ARKEMAGROUP.COM

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991