  RILSAN BECN O TL | PA11 | ARKEMA
Product Texts
DESIGATION ISO 1874-PA11,KHL,14-010
 RILSAN PA11 :
 produced from a renewable source

 Rigid grade for sheathing of wires and cables.
 Available colour : natural.
 Light and heat stabilized.

 High abrasion resistance.
 Well adapted melt viscosity.
 Ability to be processed in thin wall thickness.

 UL classification : UL94 V2 (3mm) RTI : 65/65/65

 Example applications : Coating of electrical and telephone cables,
 loose tubes for optical fiber.
Rheological propertiesdry / condUnitTest Standard
Melt volume-flow rate (MVR) 30 / * cm³/10min ISO 1133
Temperature 235 / * °C ISO 1133
Load 2.16 / * kg ISO 1133
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 1470 / 1250 MPa ISO 527-1/-2
Yield stress 43 / 41 MPa ISO 527-1/-2
Yield strain 5 / 10 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) - / N kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) - / N kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) - / 14 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) - / 11 kJ/m² ISO 179/1eA
Puncture - maximum force (-30°C) - / 5500 N ISO 6603-2
Puncture energy (-30°C) - / 65 J ISO 6603-2
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 189 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 55 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 150 / * °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 160 / * °C ISO 306
Burning Behav. at 1.5 mm nom. thickn. V-2 / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Burning Behav. at thickness h V-2 / * class IEC 60695-11-10
Thickness tested 3.2 / * mm IEC 60695-11-10
Oxygen index 25 / * % ISO 4589-1/-2
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 3 / - - IEC 60250
Relative permittivity (1MHz) 3 / - - IEC 60250
Dissipation factor (100Hz) 274 / - E-4 IEC 60250
Dissipation factor (1MHz) 166 / - E-4 IEC 60250
Volume resistivity - / 1E12 Ohm*m IEC 60093
Surface resistivity * / 1E14 Ohm IEC 60093
Electric strength - / 30 kV/mm IEC 60243-1
Comparative tracking index * / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 1.9 / * % Sim. to ISO 62
Density 1030 / 1030 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 270 °C ISO 294
Injection Molding, mold temperature 50 °C ISO 10724
Injection Molding, pressure at hold 16 MPa ISO 294
Diagrams
Viscosity-shear rate , RILSAN BECN O TL, PA11, ARKEMA
Shearstress-shear rate , RILSAN BECN O TL, PA11, ARKEMA
Stress-strain , RILSAN BECN O TL, PA11, ARKEMA
Secant modulus-strain , RILSAN BECN O TL, PA11, ARKEMA
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets
Additives
Lubricants
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Other extrusion

PREPROCESSING

Max water content: < 0.1  %

Notice text      :      RILSAN is delivered in sealed bags and is
                 :      ready for use.

                 :      Every opened bag of RILSAN which has not been
                 :      used within two hours must, as a precaution, be
                 :      re-dried.
                  
                 :      Drying conditions are 4 h at 80-90 °C in a
                 :      forced-air oven.

PROCESSING

Melt temperature : 190 - 250 °C
Disclaimer

This database provides the main properties of technical thermoplastics
marketed by ARKEMA.

      The information contained in this document is based on trials carried
out by our Research Centres and data selected from the literature, but
shall in no event be held to constitute or imply any warranty,
undertaking, express or implied commitment from our part.
Our format specifications define the limit of our commitment.
No liability whatsoever can be accepted by ARKEMA with regard to the
handling processing or use of the product or products concerned which
much in all cases be employed in accordance with all relevant laws
and/or regulations in force in the country or countries concerned.

For information about the other products marketed
by our company consult :
ARKEMAGROUP.COM

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991