View list of
  • All ARKEMA grades
  • All PA11 grades
  • All grades beginning with R

CAMPUS® datasheet | RILSAN BMN Y TLD


This datasheet of RILSAN BMN Y TLD from ARKEMA is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  RILSAN BMN Y TLD | PA11... | ARKEMA
Product Texts
DESIGNATION ISO 1874- PA11,MHLS,12-020,MD02
 
 RILSAN PA11 :
 produced from a renewable source

 Rigid grade with molybdenum filler for injection moulding.
 Available colour : steel grey.
 Light and heat stabilized.
 Mold release agent.

 No need of lubricant.
 Low friction coefficient. Abrassion resistance.
 Outstanding mechanical properties.
 Easy filling of the mold due to its well adapted melt viscosity.
 Low shrinkage : include 1% on average for the design of the mold.
 Very good dimensionnal stability (low moisture absorption).

 UL classification : UL94 V2 (3,05mm)  RTI(C) 105/90/105

 Example applications : Moving mechanical parts with friction 
 such as gear or bearing.
Rheological propertiesdry / condUnitTest Standard
Melt volume-flow rate (MVR) 36 / * cm³/10min ISO 1133
Temperature 235 / * °C ISO 1133
Load 2.16 / * kg ISO 1133
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 1490 / 1420 MPa ISO 527-1/-2
Yield stress 46 / 40 MPa ISO 527-1/-2
Yield strain 19 / 18 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 189 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 50 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 155 / * °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 162 / * °C ISO 306
Burning Behav. at 1.5 mm nom. thickn. V-2 / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Burning Behav. at thickness h V-2 / * class IEC 60695-11-10
Thickness tested 3.2 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Relative permittivity (100Hz) 4 / - - IEC 60250
Relative permittivity (1MHz) 3 / - - IEC 60250
Dissipation factor (100Hz) 545 / - E-4 IEC 60250
Dissipation factor (1MHz) 212 / - E-4 IEC 60250
Volume resistivity - / 1E12 Ohm*m IEC 60093
Surface resistivity * / 1E14 Ohm IEC 60093
Electric strength - / 55 kV/mm IEC 60243-1
Comparative tracking index * / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 1.9 / * % Sim. to ISO 62
Density 1050 / 1050 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 270 °C ISO 294
Injection Molding, mold temperature 50 °C ISO 10724
Injection Molding, pressure at hold 16 MPa ISO 294
Diagrams
Stress-strain , RILSAN BMN Y TLD, PA11..., ARKEMA
Secant modulus-strain , RILSAN BMN Y TLD, PA11..., ARKEMA
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding

PREPROCESSING

Max water content: < 0.1  %

Notice text      :      RILSAN is delivered in sealed bags and is
                 :      ready for use.

                 :      Every opened bag of RILSAN which has not been
                 :      used within two hours must, as a precaution, be
                 :      re-dried.
                  
                 :      Drying conditions are 4 h at 80-90 °C in a
                 :      forced-air oven.

PROCESSING

Melt temperature : 200 - 250 °C
Disclaimer

This database provides the main properties of technical thermoplastics
marketed by ARKEMA.

      The information contained in this document is based on trials carried
out by our Research Centres and data selected from the literature, but
shall in no event be held to constitute or imply any warranty,
undertaking, express or implied commitment from our part.
Our format specifications define the limit of our commitment.
No liability whatsoever can be accepted by ARKEMA with regard to the
handling processing or use of the product or products concerned which
much in all cases be employed in accordance with all relevant laws
and/or regulations in force in the country or countries concerned.

For information about the other products marketed
by our company consult :
ARKEMAGROUP.COM

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991