Product Texts
DESIGNATION ISO 1874-PA MACM14,MT,12-010
 Rilsan Clear.com
 Cyclo-aliphatic polyamide (PACA) grade for injection moulding.
 
 Transparency even thick.

 Excellent flexibility.
 High elasticity.
 Lightness.
 Better Processing.
 Good thermal properties.
 Good chemical resistance.
 Dimensionnal stability.

 Example applications : Glasse frames.
Rheological propertiesdry / condUnitTest Standard
Melt volume-flow rate (MVR) 6 / * cm³/10min ISO 1133
Temperature 275 / * °C ISO 1133
Load 2.16 / * kg ISO 1133
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus - / 1420 MPa ISO 527-1/-2
Yield stress - / 51 MPa ISO 527-1/-2
Yield strain - / 8 % ISO 527-1/-2
Nominal strain at break >50 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) - / N kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) N / N kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) - / 10 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) - / 11 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Glass transition temperature (10°C/min) 145 / * °C ISO 11357-1/-2
Temp. of deflection under load (1.80 MPa) 94 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 122 / * °C ISO 75-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Burning Behav. at thickness h V-2 / * class IEC 60695-11-10
Thickness tested 3.2 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Volume resistivity - / 1E11 Ohm*m IEC 60093
Surface resistivity * / 1E12 Ohm IEC 60093
Other propertiesdry / condUnitTest Standard
Water absorption 3 / * % Sim. to ISO 62
Humidity absorption 1.1 / * % Sim. to ISO 62
Density - / 990 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 280 °C ISO 294
Injection Molding, mold temperature 60 °C ISO 10724
Diagrams
Viscosity-shear rate , RILSAN CLEAR G350, PA*, ARKEMA
Shearstress-shear rate , RILSAN CLEAR G350, PA*, ARKEMA
Dynamic Tensile modulus-temperature , RILSAN CLEAR G350, PA*, ARKEMA
Stress-strain , RILSAN CLEAR G350, PA*, ARKEMA
Secant modulus-strain , RILSAN CLEAR G350, PA*, ARKEMA
Specific volume-temperature (pvT) , RILSAN CLEAR G350, PA*, ARKEMA
Characteristics
Processing
Injection Molding, Other Extrusion
Delivery form
Pellets
Special Characteristics
Transparent
Regional Availability
Disclaimer

This database provides the main properties of technical thermoplastics
marketed by ARKEMA.

      The information contained in this document is based on trials carried
out by our Research Centres and data selected from the literature, but
shall in no event be held to constitute or imply any warranty,
undertaking, express or implied commitment from our part.
Our format specifications define the limit of our commitment.
No liability whatsoever can be accepted by ARKEMA with regard to the
handling processing or use of the product or products concerned which
much in all cases be employed in accordance with all relevant laws
and/or regulations in force in the country or countries concerned.

For information about the other products marketed
by our company consult :
ARKEMAGROUP.COM

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991