  Rynite® 540SUV BK544 | PET-GF40 | DuPont Engineering Polymers
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 3 cm³/10min ISO 1133
Temperature 280 °C ISO 1133
Load 2.16 kg ISO 1133
Molding shrinkage (parallel) 0.2 % ISO 294-4, 2577
Molding shrinkage (normal) 0.9 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 13000 MPa ISO 527-1/-2
Stress at break 160 MPa ISO 527-1/-2
Strain at break 2.6 % ISO 527-1/-2
Charpy impact strength (+23°C) 50 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 9 kJ/m² ISO 179/1eA
Puncture - maximum force (+23°C) 770 N ISO 6603-2
Puncture energy (+23°C) 4.7 J ISO 6603-2
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 249 °C ISO 11357-1/-3
Coeff. of linear therm. expansion (parallel) 17 E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion (normal) 75 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm IEC 60695-11-10
Electrical propertiesValueUnitTest Standard
Electric strength 30 kV/mm IEC 60243-1
Other propertiesValueUnitTest Standard
Water absorption 0.6 % Sim. to ISO 62
Humidity absorption 0.15 % Sim. to ISO 62
Density 1640 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 1440 kg/m³ -
Thermal conductivity of melt 0.28 W/(m K) -
Spec. heat capacity melt 1760 J/(kg K) -
Ejection temperature 165 °C -
Diagrams
Viscosity-shear rate , Rynite® 540SUV BK544, PET-GF40, DuPont
Shearstress-shear rate , Rynite® 540SUV BK544, PET-GF40, DuPont
Stress-strain , Rynite® 540SUV BK544, PET-GF40, DuPont
Secant modulus-strain , Rynite® 540SUV BK544, PET-GF40, DuPont
Specific volume-temperature (pvT) , Rynite® 540SUV BK544, PET-GF40, DuPont
Tensile modulus-temperature , Rynite® 540SUV BK544, PET-GF40, DuPont
LTHA-Stress at Break 4mm, Rynite® 540SUV BK544, PET-GF40, DuPont
LTHA-Strain at Break 4mm, Rynite® 540SUV BK544, PET-GF40, DuPont
LTHA-Electric Strength 1mm, Rynite® 540SUV BK544, PET-GF40, DuPont
Characteristics
Processing
Injection Molding, Profile Extrusion
Delivery form
Pellets
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather
Regional Availability
Other text information
Injection molding

PREPROCESSING


Drying Recommended = Yes
Drying Temperature = 120°C
Drying Time, Dehumidified Dryer = 4h
Processing Moisture Content = <0.02 %


PROCESSING


Melt Temperature Optimum = 285°C
Melt Temperature Range = 280-300°C
Mold Temperature Optimum = 110°C
Mold Temperature Range = >95°C


Moulding guide

Disclaimer

E.I. du Pont de Nemours and Company is pleased to provide information about its products with the CAMPUS electronic database.

The information provided is gratis and DuPont assumes no obligation or liability for any advice furnished or for any results obtained with respect to this information.

All such advice is given and accepted at the risk of the buyer. The disclosure of information herein is not an express or implied license to operate under any patent of DuPont or others.

DuPont warrants that the use or sale of any material which is described herein and is offered for sale by DuPont does not infringe any patent covering the material itself, but does not warrant against infringement by reason of the use thereof in combination with other materials or the operation of any process.

Unless otherwise noted, the property values are for natural color (NC010) resins only. Colorants or other additives may alter some or all of the properties.
The data listed herein fall within the normal range of product properties and they should not be used to establish specification limits nor used alone as the basis of design.

Material Safety Data Sheets (SDSs) can be obtained from local sales offices.

Products listed herein should not be used in medical applications involving permanent implantation in the human body or contact with internal body fluids or tissues unless the material has been provided from DuPont under a written contract that is consistent with DuPont policy regarding medical applications and expressly acknowledges the contemplated use.

For further information, please contact your DuPont representative.

You may also request a copy of DuPont policy regarding medical applications H-50103-2 and DuPont caution regarding medical applications H-50102-2.

Products listed herein may from time to time be modified or removed.
Please call your local sales office to determine current availability.


The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991