offers extended functionality!CAMPUS® datasheet | SCHULAMID® 6 GF 30 HI K1886
This datasheet of SCHULAMID® 6 GF 30 HI K1886 from A. Schulman GmbH is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
SCHULAMID® 6 GF 30 HI K1886 | PA6-I-GF30 | A. Schulman GmbH
Product Texts
30% glass fibre reinforced PA 6 grade with increased impact; customer related compound
| Rheological properties | dry / cond | Unit | Test Standard |
| Molding shrinkage (parallel) | 0.6 / * | % | ISO 294-4, 2577 |
| Molding shrinkage (normal) | 0.9 / * | % | ISO 294-4, 2577 |
| Mechanical properties | dry / cond | Unit | Test Standard |
| Tensile Modulus | 9100 / - | MPa | ISO 527-1/-2 |
| Stress at break | 170 / - | MPa | ISO 527-1/-2 |
| Strain at break | 3.5 / - | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | 85 / - | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 16 / - | kJ/m² | ISO 179/1eA |
| Thermal properties | dry / cond | Unit | Test Standard |
| Temp. of deflection under load (1.80 MPa) | 190 / * | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 200 / * | °C | ISO 75-1/-2 |
| Vicat softening temperature (50°C/h 50N) | 200 / * | °C | ISO 306 |
| Burning Behav. at 1.5 mm nom. thickn. | HB / * | class | IEC 60695-11-10 |
| Thickness tested | 1.5 / * | mm | IEC 60695-11-10 |
| Electrical properties | dry / cond | Unit | Test Standard |
| Relative permittivity (100Hz) | 4.2 / 4.2 | - | IEC 60250 |
| Relative permittivity (1MHz) | 4 / 4 | - | IEC 60250 |
| Dissipation factor (100Hz) | 0.009 / 0.009 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | 0.02 / 0.02 | E-4 | IEC 60250 |
| Volume resistivity | >1E13 / 1E10 | Ohm*m | IEC 60093 |
| Surface resistivity | * / >1E15 | Ohm | IEC 60093 |
| Comparative tracking index | - / 550 | - | IEC 60112 |
| Other properties | dry / cond | Unit | Test Standard |
| Humidity absorption | 1.9 / * | % | Sim. to ISO 62 |
| Density | 1350 / - | kg/m³ | ISO 1183 |
| Rheological calculation properties | Value | Unit | Test Standard |
| Thermal conductivity of melt | 0.025 | W/(m K) | - |
| Eff. thermal diffusivity | 8E-8 | m²/s | - |
| Ejection temperature | 110 | °C | - |
Characteristics
Processing
Injection Molding
Delivery form
Granules
Additives
Release agent, Plasticizer
Regional Availability
Other text information
Injection molding
Pretreatment
Predrying: 4-6h / 80°C
Predrying: 4-6h / 80°C
Processing:
| Melttemperature | 250 - 280 | °C |
| Mouldtemperature | 60 - 90 | °C |
Disclaimer
The properties given in this software are typical, non-binding
mean values found fpor injection moulded natural coloured test
bars. Pigments and other modification may alter these values.
The characteristic values are based on our know-how and experience.
They do not warrant any specific properties. All our products
must be subjected to in house tests and inspections by the user
before application. This applies above all with regard to their
suitability for a particular purpose. It also applies accordingly
for all other written or verbal information given by our personnel.
Our General Terms of Business apply in all other respects,
particulaly with regard to liability for material defects.
If there are questions to given information, to further
properties or further A. Schulman products please contact
A. Schulman GmbH
Huettenstrasse 211
50170 Kerpen
Tel: 02273 / 561-0
Contact: Dipl.-Ing. M. Berg
aschulman@de.aschulman.com
Subject: Material data
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.