This datasheet of Technyl® A 218 V25 Nat BA from Rhodia Polyamide Engineering Plastics is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Technyl® A 218 V25 Nat BA | PA66-GF25 | Rhodia Polyamide Engineering Plastics
Product Texts
Polyamide 66, reinforced with 25% of glass fibre, specially stabilized to improve its resistance to oils and greases, for injection moulding.

 

TECHNYL® A 218 V25  NAT BA is recommended for mould parts exposed to high temperatures and in contact with oils and greases. Bearing housings are a typical example for which this formulation is suitable.

 

This product is approved by major bearing manufacturers.

 

This product is available in natural.

Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 262 / * °C ISO 11357-1/-3
Coeff. of linear therm. expansion (normal) 27 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
UL recognition UL / * - -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm IEC 60695-11-10
UL recognition UL / * - -
Oxygen index 23 / * % ISO 4589-1/-2
Characteristics
Processing
Injection Molding
Regional Availability
Other text information
Injection molding
The material is supplied in airtight bags, ready for use. In the case that the virgin material has absorbed moisture, it must be dried to a final moisture content of less than 0,2% with a dehumidified air drying equipment at 80~100°C

 

Recommended moulding conditions:

 

Barrel temperatures :

 

- feed zone                     260 - 270°C

- compression zone         270 - 280°C

- front zone                     280 - 290°C

 

Mould temperatures : 80-100°C

Disclaimer
WARRANTY

 This information is supplied to assist you in your choice of the
 material best suited to your requirements and does not in any way
 constitute a product specification.

 The values given relate to unpigmented materials (natural colour).
 Pigmentation can alter results. The characteristics supplied are
 typical values. Our specialists are available to advise you on the
 values to be used in order to carry out calculations correctly on
 part dimensions.

 The information contained in this document is supplied in good
 faith. However it is given purely as an indication. It shall not be
 considered in any way as a formal commitment or warranty on our part,
 notably in respect of the eventual infringement of any rights of
 third parties who may use our products. We remain at your entire
 disposal to provide you with any information that you might require.


The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991