FREE DOWNLOAD
Interested inCreating a Property Table?
The CAMPUS desktop version
offers extended functionality!CAMPUS® datasheet | Technyl® A 402 Natural FA
This datasheet of Technyl® A 402 Natural FA from Rhodia Polyamide Engineering Plastics is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
TECHNYL® A 402 NATURAL FA offers three main advantages: high impact resistance at low humidity levels, good rigidity, and excellent compression resistance.
This grade is particularly suitable for the moulding of plastic insulators for railway binding and for extrusion of plates and profiles.
Suitable for food contact applications (films, packaging, …).
This product is available in natural.
| Mechanical properties | dry / cond | Unit | Test Standard |
| Tensile Modulus | 3100 / 1300 | MPa | ISO 527-1/-2 |
| Yield stress | 80 / 60 | MPa | ISO 527-1/-2 |
| Yield strain | 8 / 30 | % | ISO 527-1/-2 |
| Charpy impact strength (+23°C) | N / N | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 7 / 30 | kJ/m² | ISO 179/1eA |
| Thermal properties | dry / cond | Unit | Test Standard |
| Melting temperature (10°C/min) | 263 / * | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 75 / * | °C | ISO 75-1/-2 |
| Coeff. of linear therm. expansion (normal) | 70 / * | E-6/K | ISO 11359-1/-2 |
| Oxygen index | 27 / * | % | ISO 4589-1/-2 |
| Electrical properties | dry / cond | Unit | Test Standard |
| Dissipation factor (1MHz) | 200 / 1000 | E-4 | IEC 60250 |
| Volume resistivity | 1E13 / 1E10 | Ohm*m | IEC 60093 |
| Surface resistivity | * / 1E12 | Ohm | IEC 60093 |
| Electric strength | 27 / 26 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 600 / 600 | - | IEC 60112 |
| Other properties | dry / cond | Unit | Test Standard |
| Water absorption | 1.5 / * | % | Sim. to ISO 62 |
| Density | 1140 / - | kg/m³ | ISO 1183 |
| Material specific properties | dry / cond | Unit | Test Standard |
| Viscosity number | 438 / * | cm³/g | ISO 307, 1157, 1628 |
The material is supplied in airtight bags, ready for use. In the case that the virgin material has absorbed moisture, it must be dried to a final moisture content of less than 0,1% with a dehumidified air drying equipment at approx 80°C.
Recommended extrusion conditions :
Barrel temperatures :
- feed zone 240 - 250°C
- compression zone 2 40 - 260°C
- front zone 240 - 260°C
Draw - plate temperatures : 260 at 270°C
Recommended extrusion conditions :
Barrel temperatures :
- feed zone 240 - 250°C
- compression zone 240 - 260 °C
- front zone 240 - 260°C
Draw - plate temperatures : 260 at 270°C
Recommended extrusion conditions :
Barrel temperatures :
- feed zone 240 - 250°C
- compression zone 240 - 260 °C
- front zone 240 - 260°C
Draw - plate temperatures : 260 at 270°C
WARRANTY This information is supplied to assist you in your choice of the material best suited to your requirements and does not in any way constitute a product specification. The values given relate to unpigmented materials (natural colour). Pigmentation can alter results. The characteristics supplied are typical values. Our specialists are available to advise you on the values to be used in order to carry out calculations correctly on part dimensions. The information contained in this document is supplied in good faith. However it is given purely as an indication. It shall not be considered in any way as a formal commitment or warranty on our part, notably in respect of the eventual infringement of any rights of third parties who may use our products. We remain at your entire disposal to provide you with any information that you might require.