View list of
  • All Rhodia grades
  • All PA666 grades
  • All grades beginning with T

CAMPUS® datasheet | Technyl® A 548B V15 Black 23N


This datasheet of Technyl® A 548B V15 Black 23N from Rhodia Polyamide Engineering Plastics is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Technyl® A 548B V15 Black 23N | PA666-GF15 | Rhodia Polyamide Engineering Plastics
Product Texts
Copolyamide 66/6, reinforced with 15% of glass fibres, heat stabilised, with a very high viscosity for blowmoulding.

 

Thanks to its processability by blow-moulding, TECHNYL® A 548B V15 BLACK 23N is suitable for the production of hollow parts like reservoirs or ducts in the automotive industry, mainly in the engine cooling and air conditioning circuits.

 

This product is available in black.

Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 5160 / 2440 MPa ISO 527-1/-2
Stress at break 100 / 58 MPa ISO 527-1/-2
Strain at break 3.9 / 13.8 % ISO 527-1/-2
Charpy impact strength (+23°C) 68 / 95 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 11 / 22 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 242 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 215 / * °C ISO 75-1/-2
Other propertiesdry / condUnitTest Standard
Density 1200 / - kg/m³ ISO 1183
Diagrams
Stress-strain , Technyl® A 548B V15 Black 23N, PA666-GF15, Rhodia
Secant modulus-strain , Technyl® A 548B V15 Black 23N, PA666-GF15, Rhodia
Characteristics
Processing
Blow Molding
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
The material is supplied in airtight bags, ready for use. In the case that the virgin material has absorbed moisture, it must be dried to a final moisture content less than 0.1% with a dehumidified air drying equipment at approx. 80°C

 

Recommended extrusion conditions:

 

- Barrel temperatures: - feed zone 250-260°C

- compression zone 260-265°C

- front zone 260-265°C

- accumulator 260-265°C

 

Die temperatures: 260-265°C

Disclaimer
WARRANTY

 This information is supplied to assist you in your choice of the
 material best suited to your requirements and does not in any way
 constitute a product specification.

 The values given relate to unpigmented materials (natural colour).
 Pigmentation can alter results. The characteristics supplied are
 typical values. Our specialists are available to advise you on the
 values to be used in order to carry out calculations correctly on
 part dimensions.

 The information contained in this document is supplied in good
 faith. However it is given purely as an indication. It shall not be
 considered in any way as a formal commitment or warranty on our part,
 notably in respect of the eventual infringement of any rights of
 third parties who may use our products. We remain at your entire
 disposal to provide you with any information that you might require.


The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991