Product Texts
Polyamide 6, 15 % glass fibre reinforced, heat stabilised
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 6100 / 2900 MPa ISO 527-1/-2
Stress at break 120 / - MPa ISO 527-1/-2
Strain at break 4 / - % ISO 527-1/-2
Charpy impact strength, +23°C 42 / - kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 5.5 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature, 10°C/min 222 / * °C ISO 11357-1/-3
Glass transition temperature, 10°C/min 55 / * °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 180 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 205 / * °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 42 / * E-6/K ISO 11359-1/-2
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 1.6 / * mm IEC 60695-11-10
Electrical propertiesdry / condUnitTest Standard
Relative permittivity, 1MHz 3.8 / 4.5 - IEC 60250
Dissipation factor, 1MHz 200 / - E-4 IEC 60250
Volume resistivity 1E13 / 1E9 Ohm*m IEC 60093
Surface resistivity * / 1E11 Ohm IEC 60093
Electric strength - / 22 kV/mm IEC 60243-1
Comparative tracking index 475 / - - IEC 60112
Other propertiesdry / condUnitTest Standard
Humidity absorption 2.55 / * % Sim. to ISO 62
Density 1220 / - kg/m³ ISO 1183
Diagrams
Viscosity-shear rate , Technyl® C 218 V15, PA6-GF15, Rhodia
Shearstress-shear rate , Technyl® C 218 V15, PA6-GF15, Rhodia
Stress-strain , Technyl® C 218 V15, PA6-GF15, Rhodia
Characteristics
Processing
Injection Molding
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PROCESSING
Melt temperature: 225°C
Mold temperature: 80°C
Disclaimer
WARRANTY

 This information is supplied to assist you in your choice of the
 material best suited to your requirements and does not in any way
 constitute a product specification.

 The values given relate to unpigmented materials (natural colour).
 Pigmentation can alter results. The characteristics supplied are
 typical values. Our specialists are available to advise you on the
 values to be used in order to carry out calculations correctly on
 part dimensions.

 The information contained in this document is supplied in good
 faith. However it is given purely as an indication. It shall not be
 considered in any way as a formal commitment or warranty on our part,
 notably in respect of the eventual infringement of any rights of
 third parties who may use our products. We remain at your entire
 disposal to provide you with any information that you might require.


The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a registered trademark of CWFG mbH, Frankfurt am Main, 2012