View list of
  • All Rhodia grades
  • All PA610 grades
  • All grades beginning with T

CAMPUS® datasheet | Technyl® eXten D 238 V30


This datasheet of Technyl® eXten D 238 V30 from Rhodia Polyamide Engineering Plastics is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

This datasheet includes:

  Technyl® eXten D 238 V30 | PA610-I-GF30 | Rhodia Polyamide Engineering Plastics
Product Texts
TECHNYL® eXten D 238 V30 is a PA6,10 30% glass fibre reinforced and impact modified suitable for injection moulding.

TECHNYL® eXten D 238 V30 is based on a partially bio-sourced polyamide 6,10.

Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.5 / * % ISO 294-4, 2577
Molding shrinkage (normal) 0.6 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 7400 / 5200 MPa ISO 527-1/-2
Stress at break 120 / 90 MPa ISO 527-1/-2
Strain at break 5 / 8 % ISO 527-1/-2
Charpy impact strength (+23°C) 90 / - kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 90 / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 27 / 31 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 15 / 18 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 215 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 190 / * °C ISO 75-1/-2
Thickness tested 1.6 / * mm IEC 60695-11-10
UL recognition UL / * - -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Other propertiesdry / condUnitTest Standard
Water absorption 1.6 / * % Sim. to ISO 62
Humidity absorption 0.34 / * % Sim. to ISO 62
Density 1250 / - kg/m³ ISO 1183
Diagrams
Stress-strain , Technyl® eXten D 238 V30, PA610-I-GF30, Rhodia
Stress-strain , Technyl® eXten D 238 V30, PA610-I-GF30, Rhodia
Secant modulus-strain , Technyl® eXten D 238 V30, PA610-I-GF30, Rhodia
Secant modulus-strain , Technyl® eXten D 238 V30, PA610-I-GF30, Rhodia
Other text information
Injection molding
The material is supplied in airtight bags, ready for use. In the case that the virgin material has absorbed moisture, it must be dried to a final moisture content less than 0,2% with a dehumidified air drying equipment at approximately

80°C.

 

Recommended moulding conditions:

 

-Barrel temperatures

Feed zone                  225-230°C

Compression zone     230-240°C

Front zone                 240-250°C

 

-Mould temperatures   80-100°C

Disclaimer
WARRANTY

 This information is supplied to assist you in your choice of the
 material best suited to your requirements and does not in any way
 constitute a product specification.

 The values given relate to unpigmented materials (natural colour).
 Pigmentation can alter results. The characteristics supplied are
 typical values. Our specialists are available to advise you on the
 values to be used in order to carry out calculations correctly on
 part dimensions.

 The information contained in this document is supplied in good
 faith. However it is given purely as an indication. It shall not be
 considered in any way as a formal commitment or warranty on our part,
 notably in respect of the eventual infringement of any rights of
 third parties who may use our products. We remain at your entire
 disposal to provide you with any information that you might require.


The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.