This datasheet includes:

  Ultradur® B 4330 G6 HR | PBT-I-GF30 | BASF
Product Texts
Injection-moulding grade with 30% glass-fibres, for rigid,tough and dimensionally stable technical parts with increased requirements on hydrolysis resistance and toughness. For example automotive connectors and housings for electronic units under the hood.

Abbreviated designation according to ISO 1043-1: PBT-I
CLASSIFICATION ACCORDING TO ISO 7792-1:
Moulding Compound ISO 7792-PBT, MGHLPRW, 11-080, GF30
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 45 cm³/10min ISO 1133
Temperature 250 °C ISO 1133
Load 10 kg ISO 1133
Molding shrinkage (parallel) 0.5 % ISO 294-4, 2577
Molding shrinkage (normal) 1.1 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 8500 MPa ISO 527-1/-2
Stress at break 120 MPa ISO 527-1/-2
Strain at break 3.4 % ISO 527-1/-2
Charpy impact strength (+23°C) 74 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 60 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 14 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 223 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 205 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 220 °C ISO 75-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Other propertiesValueUnitTest Standard
Water absorption 0.4 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1490 kg/m³ ISO 1183
Material specific propertiesValueUnitTest Standard
Viscosity number 108 cm³/g ISO 307, 1157, 1628
Diagrams
Stress-strain , Ultradur® B 4330 G6 HR, PBT-I-GF30, BASF
Secant modulus-strain , Ultradur® B 4330 G6 HR, PBT-I-GF30, BASF
Tensile modulus-temperature , Ultradur® B 4330 G6 HR, PBT-I-GF30, BASF
Characteristics
Processing
Injection Molding
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 250 - 280 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 60 - 100 °C
injection molding, Mold temperature, recommended: 80 °C
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991