View list of
Comparing
Grades?
FREE DOWNLOAD
Interested inComparing
Grades?
The CAMPUS desktop version
offers extended functionality!CAMPUS® datasheet | Ultradur® B 4500 FC
This datasheet of Ultradur® B 4500 FC from BASF is provided by the international plastics database CAMPUS.
CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.
You may contact the supplier for more information about this grade.
Ultradur® B 4500 FC | PBT | BASF
Product Texts
The BASF Ultradur® FC (Food Contact) grades enable the industry to develop products for food contact applications which are in compliance with multiple regional food contact regulations including FDA, European Food Contact n°2002/72/EC and GMP (EC) n°2023/2006.
Additional food contact compliances may also be available. Please contact your local representative or plastics safety (E-Mail: plastics.safety@basf.com, Fax: +49 621-60-93253).
Abbreviated designation according to ISO 1043-1: PBT
CLASSIFICATION ACCORDING TO ISO 7792-1:
Moulding Compound ISO 7792-PBT, E+F+MGHLN, 13-030
Additional food contact compliances may also be available. Please contact your local representative or plastics safety (E-Mail: plastics.safety@basf.com, Fax: +49 621-60-93253).
Abbreviated designation according to ISO 1043-1: PBT
CLASSIFICATION ACCORDING TO ISO 7792-1:
Moulding Compound ISO 7792-PBT, E+F+MGHLN, 13-030
| Rheological properties | Value | Unit | Test Standard |
| Melt volume-flow rate (MVR) | 19 | cm³/10min | ISO 1133 |
| Temperature | 250 | °C | ISO 1133 |
| Load | 2.16 | kg | ISO 1133 |
| Molding shrinkage (parallel) | 1.6 | % | ISO 294-4, 2577 |
| Molding shrinkage (normal) | 1.9 | % | ISO 294-4, 2577 |
| Mechanical properties | Value | Unit | Test Standard |
| Tensile Modulus | 2500 | MPa | ISO 527-1/-2 |
| Yield stress | 55 | MPa | ISO 527-1/-2 |
| Yield strain | 3.7 | % | ISO 527-1/-2 |
| Nominal strain at break | >50 | % | ISO 527-1/-2 |
| Tensile creep modulus (1h) | 1800 | MPa | ISO 899-1 |
| Tensile creep modulus (1000h) | 1200 | MPa | ISO 899-1 |
| Charpy impact strength (+23°C) | 290 | kJ/m² | ISO 179/1eU |
| Charpy notched impact strength (+23°C) | 6 | kJ/m² | ISO 179/1eA |
| Charpy notched impact strength (-30°C) | 4 | kJ/m² | ISO 179/1eA |
| Thermal properties | Value | Unit | Test Standard |
| Melting temperature (10°C/min) | 223 | °C | ISO 11357-1/-3 |
| Temp. of deflection under load (1.80 MPa) | 65 | °C | ISO 75-1/-2 |
| Temp. of deflection under load (0.45 MPa) | 165 | °C | ISO 75-1/-2 |
| Coeff. of linear therm. expansion (parallel) | 145 | E-6/K | ISO 11359-1/-2 |
| Burning Behav. at 1.5 mm nom. thickn. | HB | class | IEC 60695-11-10 |
| Thickness tested | 1.6 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Burning Behav. at thickness h | HB | class | IEC 60695-11-10 |
| Thickness tested | 0.4 | mm | IEC 60695-11-10 |
| UL recognition | UL | - | - |
| Oxygen index | 20 | % | ISO 4589-1/-2 |
| Electrical properties | Value | Unit | Test Standard |
| Relative permittivity (100Hz) | 3.3 | - | IEC 60250 |
| Relative permittivity (1MHz) | 3.3 | - | IEC 60250 |
| Dissipation factor (100Hz) | 10 | E-4 | IEC 60250 |
| Dissipation factor (1MHz) | 200 | E-4 | IEC 60250 |
| Volume resistivity | >1E13 | Ohm*m | IEC 60093 |
| Surface resistivity | 1E13 | Ohm | IEC 60093 |
| Electric strength | 36 | kV/mm | IEC 60243-1 |
| Comparative tracking index | 550 | - | IEC 60112 |
| Other properties | Value | Unit | Test Standard |
| Water absorption | 0.5 | % | Sim. to ISO 62 |
| Humidity absorption | 0.25 | % | Sim. to ISO 62 |
| Density | 1300 | kg/m³ | ISO 1183 |
| Material specific properties | Value | Unit | Test Standard |
| Viscosity number | 130 | cm³/g | ISO 307, 1157, 1628 |
| Test specimen production | Value | Unit | Test Standard |
| Injection Molding, melt temperature | 260 | °C | ISO 294 |
| Injection Molding, mold temperature | 60 | °C | ISO 10724 |
| Injection Molding, injection velocity | 200 | mm/s | ISO 294 |
Diagrams
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Other Extrusion
Delivery form
Pellets
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
injection molding, Melt temperature, range: 250 - 275 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 40 - 70 °C
injection molding, Mold temperature, recommended: 60 °C
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
injection molding, Melt temperature, range: 250 - 275 °C
injection molding, Melt temperature, recommended: 260 °C
injection molding, Mold temperature, range: 40 - 70 °C
injection molding, Mold temperature, recommended: 60 °C
Film extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
Extrusion, Flat film, Melt temperature: 230 - 280 °C
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
Extrusion, Flat film, Melt temperature: 230 - 280 °C
Other extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
Extrusion, Prepreg, Melt temperature: 230 - 250 °C
Extrusion, Pipes, Melt temperature: 230 - 260 °C
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
Extrusion, Prepreg, Melt temperature: 230 - 250 °C
Extrusion, Pipes, Melt temperature: 230 - 260 °C
Profile extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
Extrusion, Profiles, Melt temperature: 230 - 260 °C
Pre/Post-processing, max. allowed water content: .04 %
Pre/Post-processing, Pre-drying, Temperature: 80 - 120 °C
Pre/Post-processing, Pre-drying, Time: 4 h
PROCESSING
Extrusion, Profiles, Melt temperature: 230 - 260 °C
Chemical Media Resistance
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.
In order to check the availability of products please contact us or our
sales agency.
For more information about our products contact your local BASF
representative or
BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail
CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.
In order to check the availability of products please contact us or our
sales agency.
For more information about our products contact your local BASF
representative or
BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail
CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)
The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH.
M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors.
Any decision about the application of materials must be double checked with the producer of this material.
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991
CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991