This datasheet of Ultraform® H4320 Q600 from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultraform® H4320 Q600 | POM | BASF
Product Texts
High-molecular-weight grade for the extrusion of semifinished product; particularly thick walled product can be extruded at high output rates; the material also features high thermal stability and low discoloration.

Abbreviated designation according to ISO 1043: POM
Designation according to ISO 9988-1: POM-K, E-GNR, 01-002
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 2.2 cm³/10min ISO 1133
Temperature 190 °C ISO 1133
Load 2.16 kg ISO 1133
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2600 MPa ISO 527-1/-2
Yield stress 63 MPa ISO 527-1/-2
Yield strain 10 % ISO 527-1/-2
Nominal strain at break 31 % ISO 527-1/-2
Tensile creep modulus (1000h) 1300 MPa ISO 899-1
Charpy impact strength (-30°C) 180 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 6 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 5.5 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 166 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 95 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 155 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 150 °C ISO 306
Coeff. of linear therm. expansion (parallel) 110 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.6 mm IEC 60695-11-10
UL recognition UL - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
UL recognition UL - -
Oxygen index 15 % ISO 4589-1/-2
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.8 - IEC 60250
Relative permittivity (1MHz) 3.8 - IEC 60250
Dissipation factor (100Hz) 10 E-4 IEC 60250
Dissipation factor (1MHz) 50 E-4 IEC 60250
Volume resistivity 1E13 Ohm*m IEC 60093
Surface resistivity 1E13 Ohm IEC 60093
Electric strength 40 kV/mm IEC 60243-1
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.8 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1390 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Ejection temperature 110 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 200 °C ISO 294
Injection Molding, mold temperature 90 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Diagrams
Viscosity-shear rate , Ultraform® H4320 Q600, POM, BASF
Shearstress-shear rate , Ultraform® H4320 Q600, POM, BASF
Dynamic Shear modulus-temperature , Ultraform® H4320 Q600, POM, BASF
Stress-strain , Ultraform® H4320 Q600, POM, BASF
Secant modulus-strain , Ultraform® H4320 Q600, POM, BASF
Stress-strain (isochronous) 23°C, Ultraform® H4320 Q600, POM, BASF
Creep modulus-time 23°C, Ultraform® H4320 Q600, POM, BASF
Specific volume-temperature (pvT) , Ultraform® H4320 Q600, POM, BASF
Tensile modulus-temperature , Ultraform® H4320 Q600, POM, BASF
Characteristics
Processing
Injection Molding, Profile Extrusion, Sheet Extrusion, Other Extrusion
Delivery form
Pellets
Additives
Release agent
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 1 0 min
Other extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Pipes, Melt temperature: 175 - 180 °C
Profile extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Profiles, Melt temperature: 175 - 180 °C
Sheet extrusion
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
Extrusion, Plates, Melt temperature: 175 - 180 °C
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)