CAMPUS® datasheet | Ultraform® W2320 003 PRO


This datasheet of Ultraform® W2320 003 PRO from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultraform® W2320 003 PRO | POM | BASF
Product Texts
Very free-flowing, rapidly solidifying grade for use where processing is extremely difficult but mechanical properties are lower.

Ultraform® PRO offers a comprehensive service package, which supports customers in product development for the medical technology market.

Ultraform® PRO is in compliance with Pharmacopoeia and Biocompatibility-Tests in Europe, United States and Japan as specified below. However, the biocompatibility tests were recorded on tests specimens of Ultraform PRO to show compatibility of the material in general. The biocompatibility-tests listed below are not part of any continuous production control.

European Pharmacopoeia, Japanese Pharmacopoeia:
The composition of the product complies with the requirements of the European Pharmacopoeia 7th Edition, Chap. 3.2.2. "Plastic Containers and Closures for Pharmaceutical Use" and with the requirements of the Japanese Pharmacopoeia, 15th Edition, General Information, “17. Plastic Containers for Pharmaceutical Products”.
However, suitability for the end application concerned including observation of given limitations and toxicological thresholds have to be ensured on the final article by the producer.

US Pharmacopoeia: Biological Reactivity Tests, USP Plastic Class VI (USP VI)

ISO 10993-5: Biological Evaluation of Medical Devices Part 5: Test for Cytotoxicity

DMF: A Drug Master File (DMF) has been registered at FDA for Ultraform® PRO.

Food Contact: Ultraform® PRO is in compliance with multiple regional food contact regulations, especially for Europe and United States.

Additional compliances may also be available. Please contact your local representative or the Ultraplaste Infopoint (E-Mail: ultraplaste.infopoint@basf.com, Telefon: +49 621-60-78780, Fax: +49 621-60-78730).

For notice:
However, BASF has not designed or tested its plastics with respect to all of the special requirements related to their use in medical devices (defined in risk classes I to III according to the European and US Medical Device legislation) and pharmaceutical applications. Therefore BASF makes no warranties, express or implied, concerning the suitability of any BASF plastics for use in any medical device and pharmaceutical applications.

Abbreviated designation according to ISO 1043: POM
Designation according to ISO 9988-1: POM-K, M-GNR, 05-002
Rheological propertiesValueUnitTest Standard
Melt volume-flow rate (MVR) 25 cm³/10min ISO 1133
Temperature 190 °C ISO 1133
Load 2.16 kg ISO 1133
Molding shrinkage (parallel) 2.0 % ISO 294-4, 2577
Molding shrinkage (normal) 2.1 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
Tensile Modulus 2800 MPa ISO 527-1/-2
Yield stress 65 MPa ISO 527-1/-2
Yield strain 7.5 % ISO 527-1/-2
Nominal strain at break 24 % ISO 527-1/-2
Tensile creep modulus (1h) 2100 MPa ISO 899-1
Tensile creep modulus (1000h) 1350 MPa ISO 899-1
Charpy impact strength (+23°C) 150 kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 150 kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 5 kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 4 kJ/m² ISO 179/1eA
Thermal propertiesValueUnitTest Standard
Melting temperature (10°C/min) 167 °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 100 °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 156 °C ISO 75-1/-2
Vicat softening temperature (50°C/h 50N) 150 °C ISO 306
Coeff. of linear therm. expansion (parallel) 110 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.6 mm IEC 60695-11-10
UL recognition UL - -
Burning Behav. at thickness h HB class IEC 60695-11-10
Thickness tested 0.8 mm IEC 60695-11-10
UL recognition UL - -
Oxygen index 15 % ISO 4589-1/-2
Electrical propertiesValueUnitTest Standard
Relative permittivity (100Hz) 3.8 - IEC 60250
Relative permittivity (1MHz) 3.8 - IEC 60250
Dissipation factor (100Hz) 10 E-4 IEC 60250
Dissipation factor (1MHz) 50 E-4 IEC 60250
Volume resistivity 1E13 Ohm*m IEC 60093
Surface resistivity 1E13 Ohm IEC 60093
Electric strength 40 kV/mm IEC 60243-1
Comparative tracking index 600 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.8 % Sim. to ISO 62
Humidity absorption 0.2 % Sim. to ISO 62
Density 1400 kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Ejection temperature 110 °C -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 200 °C ISO 294
Injection Molding, mold temperature 90 °C ISO 10724
Injection Molding, injection velocity 200 mm/s ISO 294
Diagrams
Viscosity-shear rate , Ultraform® W2320 003 PRO, POM, BASF
Shearstress-shear rate , Ultraform® W2320 003 PRO, POM, BASF
Dynamic Shear modulus-temperature , Ultraform® W2320 003 PRO, POM, BASF
Stress-strain , Ultraform® W2320 003 PRO, POM, BASF
Secant modulus-strain , Ultraform® W2320 003 PRO, POM, BASF
Stress-strain (isochronous) 23°C, Ultraform® W2320 003 PRO, POM, BASF
Creep modulus-time 23°C, Ultraform® W2320 003 PRO, POM, BASF
Stress-strain (isochronous) 40°C, Ultraform® W2320 003 PRO, POM, BASF
Creep modulus-time 40°C, Ultraform® W2320 003 PRO, POM, BASF
Stress-strain (isochronous) 60°C, Ultraform® W2320 003 PRO, POM, BASF
Creep modulus-time 60°C, Ultraform® W2320 003 PRO, POM, BASF
Stress-strain (isochronous) 80°C, Ultraform® W2320 003 PRO, POM, BASF
Creep modulus-time 80°C, Ultraform® W2320 003 PRO, POM, BASF
Stress-strain (isochronous) 100°C, Ultraform® W2320 003 PRO, POM, BASF
Creep modulus-time 100°C, Ultraform® W2320 003 PRO, POM, BASF
Stress-strain (isochronous) 120°C, Ultraform® W2320 003 PRO, POM, BASF
Creep modulus-time 120°C, Ultraform® W2320 003 PRO, POM, BASF
Specific volume-temperature (pvT) , Ultraform® W2320 003 PRO, POM, BASF
Tensile modulus-temperature , Ultraform® W2320 003 PRO, POM, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .2 %
Pre/Post-processing, Pre-drying, Temperature: 100 °C
Pre/Post-processing, Pre-drying, Time: 3 h

PROCESSING
injection molding, Melt temperature, range: 190 - 230 °C
injection molding, Melt temperature, recommended: 200 °C
injection molding, Mold temperature, range: 60 - 120 °C
injection molding, Mold temperature, recommended: 90 °C
injection molding, Dwell time, thermoplastics: 1 0 min

Processing

Usual single-flighted three-section screws with an effective screw length of at least 15 D, better 20 - 23 D are suitable for the injection molding of Ultraform.

Pretreatment

Granules or pellets in original packaging can be processed without any special pretreatment. Granules or pellets which have become moist due to prolonged or incorrect storage (e.g. by formation of condensed water) must be dried in dehumidifying or recirculating air dryers for approx. 3 hours at about 100 - 110 °C. The moisture content should not exceed 0.2 %.


Postprocessing
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991