CAMPUS® datasheet | Ultramid® 8202 HS


This datasheet of Ultramid® 8202 HS from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultramid® 8202 HS | PA6 | BASF
Product Texts
Ultramid® 8202 HS is a heat stabilized, low viscosity, general purpose Polyamid 6 injection molding.
It possesses the combination of strength and toughness and has excellent chemical and abrasion resistance. The heat stabilizer system extends the retention of properties at the more elevated temperatures. Excellent in filling thin walls or areas.

Ultramid® 8202 HS is generally recommended for drapery hardware, gears, fittings, furniture casters, bearings, handles, clips, fasteners and thin parts.
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 2700 / 970 MPa ISO 527-1/-2
Yield stress 78 / 36 MPa ISO 527-1/-2
Yield strain 4 / 16 % ISO 527-1/-2
Nominal strain at break 25 / >50 % ISO 527-1/-2
Charpy impact strength (+23°C) N / - kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 51 / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 3.5 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 220 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 60 / * °C ISO 75-1/-2
Burning Behav. at thickness h V-2 / * class IEC 60695-11-10
Thickness tested 0.7 / * mm IEC 60695-11-10
UL recognition UL / * - -
Electrical propertiesdry / condUnitTest Standard
Volume resistivity >1E13 / - Ohm*m IEC 60093
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 9.5 / * % Sim. to ISO 62
Humidity absorption 2.7 / * % Sim. to ISO 62
Density 1130 / * kg/m³ ISO 1183
Rheological calculation propertiesValueUnitTest Standard
Density of melt 932 kg/m³ -
Thermal conductivity of melt 0.264 W/(m K) -
Spec. heat capacity melt 3730 J/(kg K) -
Test specimen productionValueUnitTest Standard
Injection Molding, melt temperature 260 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 10724
Diagrams
Viscosity-shear rate , Ultramid® 8202 HS, PA6, BASF
Shearstress-shear rate , Ultramid® 8202 HS, PA6, BASF
Dynamic Shear modulus-temperature , Ultramid® 8202 HS, PA6, BASF
Stress-strain , Ultramid® 8202 HS, PA6, BASF
Secant modulus-strain , Ultramid® 8202 HS, PA6, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
North America
Other text information
Injection molding
PREPROCESSING
Max. Water content: 0.2%
Product is supplied in sealed containers and drying prior to molding is not required. If drying becomes necessary, a dehumidifying or desiccant dryer operating at 80 °C (176 °F) is recommended. Drying time is dependent on moisture level.
Further information concerning safe handling procedures can be obtained from the Material Safety Data Sheet. Alternatively, please contact your BASF representative.

PROCESSING
Melt Temperatur e 240-280 °C (464-536 °F)
Mold Temperature 80-95 °C (176-203 °F)
Injection and Packing Pressure 35-125 bar (500-1500 psi)

A mold temperature of 80-95 °C (176-203 °F) is recommended, but temperatures of as low as 10 °C (50 °F) can be used where applicable.

Injection pressure controls the filling of the part and should be applied for 90% of ram travel. Packing pressure affects the final part and can be used effectively in controlling sink marks and shrinkage. It should be applied and maintained until the gate area is completely frozen off.

Fast fill rates are recommended to insure uniform melt delivery to the cavity and prevent premature freezing.
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991