CAMPUS® datasheet | Ultramid® A3WG6 HRX bk 23591


This datasheet of Ultramid® A3WG6 HRX bk 23591 from BASF is provided by the international plastics database CAMPUS.

CAMPUS is organized by a group of leading international resin producers, who have agreed to test their material according to uniform conditions, based on ISO standards (ISO 10350, ISO 11403), in order to offer comparable data to the market.

You may contact the supplier for more information about this grade.

This datasheet includes:

  Ultramid® A3WG6 HRX bk 23591 | PA66-GF30 | BASF
Product Texts
Glass fibre reinforced injection moulding grade with enhanced resistance to hydrolysis and heat ageing. I.e.: for applications in the automotive cooling circuit.
Rheological propertiesdry / condUnitTest Standard
Molding shrinkage (parallel) 0.5 / * % ISO 294-4, 2577
Molding shrinkage (normal) 1.2 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
Tensile Modulus 10000 / 6100 MPa ISO 527-1/-2
Stress at break 185 / 110 MPa ISO 527-1/-2
Strain at break 3.4 / 7.2 % ISO 527-1/-2
Charpy impact strength (+23°C) 85 / - kJ/m² ISO 179/1eU
Charpy impact strength (-30°C) 70 / - kJ/m² ISO 179/1eU
Charpy notched impact strength (+23°C) 10 / - kJ/m² ISO 179/1eA
Charpy notched impact strength (-30°C) 8 / - kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
Melting temperature (10°C/min) 260 / * °C ISO 11357-1/-3
Temp. of deflection under load (1.80 MPa) 245 / * °C ISO 75-1/-2
Temp. of deflection under load (0.45 MPa) 260 / * °C ISO 75-1/-2
Other propertiesdry / condUnitTest Standard
Water absorption 5.5 / * % Sim. to ISO 62
Humidity absorption 1.7 / * % Sim. to ISO 62
Density 1360 / - kg/m³ ISO 1183
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Heat stabilized or stable to heat
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 280 - 300 °C
injection molding, Melt temperature, recommended: 290 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Disclaimer
The data contained in this publication are based on our current
knowledge and experience. In view of the many factors that may affect
processing and application of our product, these data do not relieve
processors from carrying out their own investigations and tests. Any
descriptions, drawings, photographs, data, proportions, weights etc.
given herein may change without prior information and do not constitute
the agreed contractual quality of the product. It is the responsibility
of the recipient of our products to ensure that any proprietary rights
and existing laws and legislation are observed. NO WARRANTIES OF ANY
KIND, EITHER EXPRESS OR IMPLIED, INCLUDING WARRANTIES OFMERCHANTABILITY
OR FITNESS FOR A PARTICULAR PURPOSE, ARE MADE REGARDING PRODUCTS
DESCRIBED OR DESIGNS, DATA OR INFORMATION SET FORTH, OR THAT THE
PRODUCTS, DESIGNS, DATA OR INFORMATION MAY BE USED WITHOUT INFRINGING
THEINTELLECTUAL PROPERTY RIGHTS OF OTHERS.

In order to check the availability of products please contact us or our
sales agency.


For more information about our products contact your local BASF
representative or

BASF SE
Dept. KS/KC
Fax: 0621-60-49497
e-mail: e-mail

CAMPUS® is a registered trademark of CWFG (Chemie
Wirtschaftsfoerderungsgesellschaft GmbH, Frankfurt)

The CAMPUS internet database is hosted by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

CAMPUS® is a Registered trademark of CWFG mbH, Frankfurt/Main, 1991